A356 T4 heat treatment
B. Dang et al./ Materials and Design 57 (2014) 73–78
75
solution treatment achieved. It then follows that the modi cation of eutectic Si undergoes three stages: (1) edges rounding; (2) fragmentation; and (3) coarsening. Due to the more signi cant effect of the coarsened Si after fragmentation on the mechanical properties of material, the coarse effect of eutectic Si as functi
on of solution temperature and time should be explicitly stated. On this basis, the mean size including the thickness (short rod-like) and diameter (spherical shape) of eutectic Si is statistically measured to estimate the coarsening effect of eutectic Si due to solution treatment as shown in Fig. 6. By combining with the morphologies of eutectic Si in Fig. 4, one can see that the mean size of eutectic Si increases signi cantly at 540°C for 120 min solution treatment, i.e. eutectic Si is coarsened. However, as for solution treatment at 500°C, the mean size of eutectic Si increases slightly even after 120 min solution time, i.e. eutectic Si is hardly coarsened, indicating a weakened modi cation at lower temperature. As for solution treatment at 450°C, the morphology of eutectic Si is nearly independent of the solution time, indicating an inactive movement of Si atoms at or below 450°C. On this basis, the temperature of 540°C is determined as the optimized temperature for current solution treatment, in consideration of low product cost. Applying EDS, detailed phase identi cations were performed for the sample subjected to solution treatment at 450°C for 15 min, which reveals that the phase of A and B in Fig. 4 (450°C, 15 min) may be identi ed as Mg2Si phase forming in solidi cation process and Al–Fe–Mg–Si intermetallic compound (i.e. not addressed here), respectively. In consistent with Ref.[13], the sample solution-treated at 540°C for 15 min does not contain the coarse Mg2Si, which, however, can be found in samples solution-treated at 500°C for less than 60 min and at 450°C for all the solution time. One can see, the as-cast Mg2Si can be re-dissolved in the temperature range of 500–540°C; the dissolution rate increases with the solution temperature. 3.4. Hardness tests Subjected to the solution treatment, the samples are substantially hardened. As shown in Fig. 7, the hardness values as function of the solution temperature and time indicate that, at a given solution temperature, e.g. 450°C and 500°C, the hardness increases with the solution time, and at a given solution time, the hardness and hardening rate increase with the solution temperature. However, the above rule does not hold for the solution treatment at 540°C: an abnormal decline of the hardness value takes place at Fig. 3. Typical solidi cation microstructure of A356 alloy cast by PTC method, (b) as the local magni cation of (a), showing details of micro-compositions: the eutectic Si morphology, nano-scale Si precipitates and a visible PFZ existing between eutectic Si and Al matrix.
120 min solution time, which may be attributed to the coarsening of eutectic Si (Section 3.3). Evolution of the hardness with the natural aging time is shown in Fig. 8, where the sample solution-treated at 540°C for 90 min (Fig. 8a), at 500°C for 120 min (Fig. 8b) and at 450°C for 120 min (Fig. 8c) are denoted as sample I, sample II and sample III, r
espectively. For sample III, the hardness can be determined as$105 HV regardless of the natural aging time. But for sample I and II, the hardness values both increase rstly and then remain plateau with the natural aging time; sample I needs less natural aging time ($10 h) than sample II ($23 h), to achieve the maximum hardness of$140 HV and$155 HV, respectively. So, the hardening rate of sample I is larger than that of sample II during natural aging process, which indicates strongly that the age hardening is affected signi cantly by the solution temperature and time.
4. Discussion 4.1. Forming mechanism of dendritic eutectic Si and nano-scale Si particle From Fig. 3b, dendritic eutectic Si and nano-scale Si particles can be observed in the as-cast microstructure. This phenomenon is according to Bendijk et al.[14] ascribed to the high cooling rate of solidi cation, i.e. the dendritic eutectic Si, usually occurring in
Fig. 2. Cooling curve (solid line) and solid transformed volume faction (scatter triangle) calculated by NTA method of A356 alloy in solidi cation, de nition of the‘‘post-solidi cation stage’’ as temperature below 545°C on cooling curve.

Effect of heat treatment on microstructure and ...The LMD alloy was given a solution treatment at...The hardness of the samples was measured using a...
Effect of pre post T6 heat treatment on the ...of laser welded SSM cast A356 aluminium alloy R...Microstructure, hardness and tensile properties of ...
Influence of post-weld heat treatment on the microstructure and hardness of laser weld seams on The transformation induced plasticity (TRIP) steels effect ...
b titanium alloys after different heat treatment. ...alloy microstructure, and the effect of the ...Hardness tests were carried out using a Vickers ...
Effect of yttrium on the microstructure of a semi-solid A356 Al alloy_专业资料。Avll niea\^^sineic.oaieol t^n,cecdrtm abnn.ec 喜Sinerc ...
Effect of thermomechanical treatment on microstructure and hardness behavior of AZ63 magnesium a 隐藏>> Avibeolea all ni tanwww.cecdrc.osineitm et姆 AC7 ...
effect of manganese on the microstructure and ...The surface hardness was measured by Vickers ...Brooks, Heat Treatment, Structure and Properties ...
EFFECT OF COLD ROLLING ON THE MICROSTRUCTURE AND ...The initial hardness of the alloy increased with ...heat treatment distributed along grain boundaries or...
and micro-hardness of Cu-3.5wt.%Ti-0.1wt.%Zr-RE alloy were investigated after optimizing technics of plastic deformation and the heat treatment. ...
Effect of heat treatment on plasticity of Al-Zn-Mg alloy: Microstructure ...(Hv) was measured on samples using shimadzu HVM-2000 hardness, at a load...