A356 T4 heat treatment
74B.adoptedtore neA356alloysamples.These

solutiontreatedatdifferenttemperaturesandtime,effectsofthere nedmicrostructureonthetreatment.ThiswillprovidefundamentalandcontinuousdiecastingprocessforAl-basedregardingageneralreductionofsolutionheati.e.theproductivityandmanufacturingcost.
2.Experimentalprocedure
A356alloy(Al,7.0wt.%Si,0.4wt.%Mg,0.1wt.%inaresistantfurnace,thendegassedwithshieldedbytheinertgas.Aftertwocyclesoftheliquidmeltwaskeptat680°C(about75°Cuidustemperatureof605°C)for20mintoallowuniform,andthenpouredintothecylindricalsizeof10mmdiameter,100mmlengthand3(Fig.1).APTC[9]technologywasusedtocoolmetalforrapidsolidi cation.AK-typeintothecenterofliquidinthecoppermouldtocurveuponsolidi cation;relevantdatawasColorPaperlessRecorder.
Aftercasing,thesesamplesweresubjectedtoationtreatment,1at540°C,450°Cand400°C,for60min,90minand120minfollowedby72hnaturalaging(i.e.T4heattreatment).Evolutionofthemicrostructureandhardnesswiththesolutiontemperatureandtimewasinvestigated.Theas-polishedsampleswereetchedin0.5%HFsolutionfor30storevealthestruc-turemorphologies,andfurtherobservedusingscanningelectronmicroscope(SEM)withlightelementenergydispersivespectroscopy(EDS)X-raydetectors.ThenmicrostructuralquantitativeanalysiswasperformedondeeplyetchedsamplesusingthesoftwareIMAGEJ;eachsamplewasmeasuredrepetitivelybytwentytimes,andthemeanvaluewasselected.Differentialscanningcalorimetry(DSC)wasperformedusingNETZSCHSTA409PC/PGtostudythethermalhistoryofthemeltingprocessofalloy.InDSCexperiment,10mgofthedisc-likesample(3mmdiameterand1.5mmthickness)wasprepared,and20°C/minheatingrateofand70ml/minargon uxwereperformed.Micro-hardnesstestswereaccordingtoASTM:E384–11e1standardsandperformedusingVickersmethod(SHI-MADZY,Japan).Theindentationwasmadeonthewell-polishedsur-faceofthespecimenswithadiamondsquare-basedpyramidunderaloadof9.8mNforaperiodof15s.Themeasurementswerere-peatedtentimesandthemeanvaluewascalculated.
3.Experimentalresults3.1.Coolingcurve
ThecoolingcurveofA356alloywasmeasuredbyaK-typether-mocoupleasshowninFig.2(solidline),where,threein exionsweredeterminedas605°Cforprimarya-Alsolidi cation,575°CforAl–Sieutectictransformation,and545°CforAl+Si+Mg2Siter-naryeutectictransformation.Suchdatawasalsoreportedelse-where[10].Correspondingtotheslopeofcoolingcurveabove605°C,thecoolingratewascalculatedas40°C/s.Evolutionoftheprimarya-Alphasesolidi edwiththetemperaturewascalcu-latedusingNewtonthermalanalysis(NTA)[11]asshowninFig.2(scattertriangle),wherethevolumefractionofa-Al,fa-Al,upontheprimarysolidi cationwascalculatedas$68%.Itshouldbenotedthattheas-solidi edmicrostructureiscomposedonlyofprimary
1
Thesolutiontreatmenthereisreferredtoaprocessofsolutiontreatmentfollowedbyrapidquenchingtoroomtemperature.
a-AlphaseandAl-Sieutectic,sinceMgcontentislessthan
0.5wt.%andthusignored.3.2.As-solidi edmicrostructure
Theas-solidi edmicrostructureofthesampleduetoPTCcool-ingisshowninFig.3,where,thea-AldendriteandtheAl-Sibinaryeutecticdistributedwithintheinter-dendriticnetworkarereadilyindenti ed(Fig.3a).Thesecondarydendritearmspacing(SDAS)fora-Aldendriteismeasuredas$15lm,thelengthandthicknessoflamellareutecticSiismeasuredas$15lmand$0.5lm,respectively.Asthemagni cationofthepositiondenotedbyawhiterectanglewithdashlineinFig.3aandbshowsthenano-scalesiliconparticlesuniformlydistributedwithinthea-Almatrix,andmoreover,theeutecticSiwithhacklyedgesandtheprecipi-tate-freezone(PFZ)clearlyobserved.SuchtypicalmicrostructuresassmallSDAS, neeutecticSianduniformdistributedSiprecipi-tates,aswellasfewas-castedmicro-defects[12]duetoPTCcool-ing,willcontributetotheimprovementofmechanicalproperty,e.g.thehighhardnessof$90HVachieved(Fig.5inSection3.4).3.3.Microstructureevolutionafterdifferentsolutiontreatments
Typicalmicrostructuressubjectedtodifferentsolutiontreat-mentsareshowninFig.4,where,themorphologicalevolutionofMg2SiandeutecticSiwithsolutiontemperatureandtimewerecharacterizedbySEM.Ascomparedtotheas-solidi edmicrostruc-tures,nosiliconprecipitatesarefoundinallthesolution-treatedsamples,whilstthehacklyedgesofeutecticSiarealsoclearlysmoothed(seeFig.5),andthemodi cationofeutecticSidependsonthesolutiontemperatureandtime.
Ifthesolutiontemperatureissetas540°C(Fig.4),theedgesofeutecticSiwillberoundedin15minsolutiontime,andextremelyroundedin35minsolutiontime.After60minsolutiontime,frag-mentationofeutecticSioccursandthesefragmentizedSiparticlesarecontinuouslyroundedin90minsolutiontimeandthusbecomeshort-likeorspherical-like,butoncethesolutiontimeislargerthan90min,thecoarseningofeutecticSistarts,i.e.thewell-knownOstwaldripeningcorrespondstotheoptimum
Effect of heat treatment on microstructure and ...The LMD alloy was given a solution treatment at...The hardness of the samples was measured using a...
Effect of pre post T6 heat treatment on the ...of laser welded SSM cast A356 aluminium alloy R...Microstructure, hardness and tensile properties of ...
Influence of post-weld heat treatment on the microstructure and hardness of laser weld seams on The transformation induced plasticity (TRIP) steels effect ...
b titanium alloys after different heat treatment. ...alloy microstructure, and the effect of the ...Hardness tests were carried out using a Vickers ...
Effect of yttrium on the microstructure of a semi-solid A356 Al alloy_专业资料。Avll niea\^^sineic.oaieol t^n,cecdrtm abnn.ec 喜Sinerc ...
Effect of thermomechanical treatment on microstructure and hardness behavior of AZ63 magnesium a 隐藏>> Avibeolea all ni tanwww.cecdrc.osineitm et姆 AC7 ...
effect of manganese on the microstructure and ...The surface hardness was measured by Vickers ...Brooks, Heat Treatment, Structure and Properties ...
EFFECT OF COLD ROLLING ON THE MICROSTRUCTURE AND ...The initial hardness of the alloy increased with ...heat treatment distributed along grain boundaries or...
and micro-hardness of Cu-3.5wt.%Ti-0.1wt.%Zr-RE alloy were investigated after optimizing technics of plastic deformation and the heat treatment. ...
Effect of heat treatment on plasticity of Al-Zn-Mg alloy: Microstructure ...(Hv) was measured on samples using shimadzu HVM-2000 hardness, at a load...
热门文档