J. Mater. Sci. Technol., Vol.18 No.6, 2002

Table 1 Composition and properties of Fe powders

Kinds of powders

Deoxidizing powder QMP100I

Provided by Hogonas Gas atomized powder

0 (w/o) 0.36 0.08 0.08 0.10

C S (w/o) (w/o) 0.040 0.030 0.003 0.007 0.005 0.008 0.020 0.020

P (w/o) 0.030

Fe Apparent

(w/o) density/(g/cm3)

2.30 balance

2.92 balance

2.94 balance

2.65’2.95 balance

Flowability

(50 g)/s 40 26 24.6 35

Particle size/urn 300 250 250

300

0.010

0.010 0.015

Table 2 Chemical compositions of alloys used for powder forging connecting rods

Kinds of materials

1 2 3 4

Particle size/urn

C(w/o) 0.20.5 0.30.6 0.30.6 0.3’0.6 <100

Cu(w/o)

-

Ni(w/o) Mo(w/o)

—

12 12 1-.’2 00

1.5’-’2 150

0.2r0.3 0.2’.’0.3 100

Fe(w/o) balance balance balance balance 300

Zinc stearate(w/o)

0.8 0.8 0.8 0.8

1

-

-

I

7

-

Fig.6 Powder forging die with ifash

±—upper bolster, 2—upperdie, 3 pill, 4 lower die, 5 core, 6 fix board, 7—lower bolster

Powder Forging of a Motorcycle Connecting Rod (1)

pact must be realized by fiashless forging process. rrherefore a set of flashless powder hot forging die was then desigued, as shown in Fig.7. The inclination between cavity and pil-

lar was designed for entering the sintered compact and ease of ejecting the forging. Exhaust holes on the upper bolster could prevent the high pressure air mass from affecting metal flow and damaging the die. When the ram moves upward, the ejector can eject the lower punch and the forged com-

pact together. Because the fiashless powder forging makes the compact in a three-dimensional compressive stress state and confines deformation within the die cavity, the powder forging can realize high density, smooth surfaces and required

dimensions. In addition, the fiashless forging process can pro-vide the most economic milling excess on the surface of the

pin ends and inside holes of the connecting rod. Advanced CAD/CAM technology was used to manufacture the upper and lower die cavities.

2.5 Forging process

Powder forging was performed on a 1600 kN friction screw pess. The pressure was controlled at about 1000.-’1400 MPa during forging. The initial forging temperature of the com-

pact was 1400°C. In order to protect the compacts from ox- idizing, a 4 kVA furnace was always filled with high purity N2 gas during heating. After heating for 10 miii, the compact was manually removed from the furnace and put into the hot forging die quickly. In order to avoid oxidation in cooling, the forged compact was dropped into oil directly after being ejected from the mould, The effect of the forging temperature on the forged compact density is shown in Fig.8.

Fig.T No-flash die of powder forging

1—upper bolster, 2—upper punch fix board, 3—lower punch fix board, 4—core fix board, 5—lower bolster, 6—upper punch, 7—core, 8—lower punch, 9—ejector

obtained the following results: (1) When surplus powder was over 30 w/o, the average relative density of the forged com-

pact was over 97%. Lesser amount of the surplus powder resnlted in the lower density. (2) Wheo the weight of powder did not exceed the required amount, cracks happened in the transition nrea between the two ends and the crank. This resulted from the stress of crosswise flow exceeding the mate-

rial fracture strengtk. (3) Powder forging with flash did not exploit powder forging advantages, if the powder weight is beyond the required amount, the flash emerged. If the pow-

der weight was less than the required amount, the density was very low so as to cause forging defects in the transition area. (4) When heated for 10 mm at 1000°C, the compact thermal expansion was 2,3%r.s2.5%. The shrinkage was 0.7%’.0.8% after hot forging.

The experimental results of the powder forging with flash indicated that the desired densification of the sintered com

3. Results and Discussion

Density is the main factor that affects the final mechani-

cal properties of the P/M connecting rod. In order to satisfy the practical requirements, the final density of the connecting

rod must achieve over 97% of the theoretical density. This re-quires that the compact has a uniform density and reasonable

material components. Experiments found that for the same hot forging process conditions the density of the forged P/M connecting rod was highest when the compact density was 6.4’-6.5 g/cm3, as shown in Fig.9. The lower compact density would result in the nonuniform density distribution along the height of the connecting rod. On the other hand, the high compact density would increase the densification force and forging energy significantly.

Through comparison of the physical and mechanical prop-

erties of the sintered compact and the forged compact (as shown in Table 3), Fe-C-Cu-Mo was selected as the alloy pow-

der. The detailed chemistry of the alloy powder was 0.5 w/o C, 1.-s2 w/o Cu, 0.2r-.O.6 w/o Mo, and the remainder was Fe. The microstructures of the sintering compact and the forged compact were examined by the optical microscope, as shown

上一页第3页

你可能喜欢

热门文档

相关文档

  • 制造工程与技术(热加工)英文版14 Forging of Metals

    – by forging – by casting – by powder metallurgy(粉末冶金) – by ...removing flash Figure 14.7 (a) Stages in forging a connecting rod for ...

  • 05金属锻造forging of Metals

    Costs of a Rod Made by Forging and Casting Figure 14.19 Relative unit costs of a small connecting rod made by various forging and casting processes. ...

  • Forging

    powder metallurgy or casting, or a preformed blank from a prior forging ...s shape gradually changes, as shown for the forging of a connecting rod....

  • Connecting_Batteries_and_Chargers_in_Series_and_Par...

    Powder+Forging+of+a+Mo... 暂无评价 6页 1下载券 Connecting rod is an i... 2页 免费 The Finite Element Ana... 4页 2下载券 connecting rod(曲柄连...

  • 中国连杆锻造的发展回顾

    [2] Q.L. Luo, Improved production technology of motorcycle forgings, ...Lei, New technology for precision forging of connecting rod, J. Jinan Univ...

  • 金属的锻造ForgingofMetalsCh14

    Costs of a Rod Made by Forging and Casting Figure 14.19 Relative unit costs of a small connecting rod made by various forging and casting processes. ...

  • PowderForgingofaMotorcycleConnectingRod

    PowderForgingofaMotorcycleConnectingRod 隐藏>> 5 44 J . t Ma e r . Sei . e T e hn o l厂 b l18 V . . N o . 6 , 2002 P G w o u ...

  • Diesel engine connecting rod processing

    Diesel engine connecting rod processing Abstract The connecting rod is one of...Two holes can not directly, forging Work. By looking at more than ...

  • ...Gripping Mechanism Clamping Force of Forging

    Gripping Mechanism of Forging Manipulator Structure Composition. The gripping mechanism is made up of pushing rod, connecting rod, clamp and clamping cylinder...

  • Conrod

    Conrod_机械/仪表_工程科技_专业资料。connecting rod manufacturing processJanuary...densification of a heated powder-based preform using a single forging strike...

站点地图 | 文档上传 | 侵权投诉 | 手机版
本站所有资源均来自互联网,本站只负责收集和整理,均不承担任何法律责任,如有侵权等其它行为请联系我们.
文档下载 Copyright 2013 doc.guandang.net All Rights Reserved.  -  email