TABLE 2 - MINIMUM BAKE SOAK TIMES (HOURS) ON HIGH ALLOY, ULTRA-HIGH STRENGTH STEELS,

AND FOR CASE HARDENED SURFACES

Platings

Steel/Part

(9)

Description

Specified Minimum

(1) (8)

Hardness

All

(5)

(6)

Chemical

Treatments

(3)

(4)

Bake Temperatureoo

F (C) 325 °F (163 °C)

Cd

(2)

& Ni Cd-Ti23 23 23 23

23 23 23 23

Cr 8 23 23 8

TDCr (7)

Etch 23 23 23 23

23 23 8 8

8 23 23 8

5 5 5 5

5 5 5 8

23 23 8 23

8 8 4 8

8 4 4

Music Wire 96 96 23 96

275 °F (135 °C)52100 440C Stainless

Below 62 HRC 375 °F (191 °C)46 HRC

(5)

300 °F (149 °C)NA

Carburized

All Parts 275 °F (135 °C)23 23 8 23 23 23 8 5 5 23 8 8

Carbonitrided Nitrided

All Parts 375 °F (191 °C)8 8 8 23 8 8 8 3 3 8 3 4

Nitrocarburized

NOTES:

NA - Not applicable (1) Or equivalent

(2) Includes electroless nickel unless age hardened within four hours (3) Chemical Processing: Etching, Stripping, Pickling, Chemical Milling

(4) Etch Inspection to detect abusive grinding/machining or the presence of carburizing - Baking is required after etch inspection

when hydrochloric or other reducing acid is used (e.g., AMS2649, Type 2 hydrochloric acid desmut). (5) Or higher specified minimum hardness

(6) For platings not listed, use baking time shown for cadmium. (7) Thin dense chromium plating (e.g., AMS2438).

(8) For induction hardened or carburized parts, an extended bake time in excess of 23 hours is prohibited.

(9) Other alloys – For other alloys tempered at 300 °F (149 °C) or lower, a baking schedule of 275 °F (135 °C) for 96 hours shall

be used. For other alloys tempered at 400 °F (204 °C) and hotter, a baking schedule of 375 °F (191 °C) for 23 hours shall be used. For other alloys tempered between 300 °F (149 °C) and 400 °F (204 °C), contact the cognizant engineering organization to verify the proper baking schedule.

3.3.3.6 Multistep Processes

An additional intermediate baking treatment is required if there is an interruption between steps exceeding 2 hours or if the elapsed time between the start of the first step and start of final baking exceeds 24 hours. 3.3.3.6.1 3.3.3.6.2 3.3.3.6.3 3.3.3.6.4

When the strength is 240 ksi (1655 Mpa) or lower (49 HRC or less), the intermediate bake soak time shall be 3 hours minimum, unless parts are nickel plated. See 3.3.3.6.3.

When the strength is over 240 ksi (1655 Mpa) (over 49 HRC), the intermediate bake the soak time shall be 6 hours minimum, unless parts are nickel plated. See 3.3.3.6.3.

When parts are nickel plated and heat treated to 200 ksi (1379 Mpa) or higher (43 HRC or harder), the intermediate bake soak time shall be the full amount of time shown in Table 1 or 2, as applicable.

After completion of the final step of chemical treatment or plating, full baking in accordance with applicable Table 1 or 2 is required.

3.4 Records

Records shall be maintained that show the identification and the following for each lot: 3.4.1 3.4.2 3.4.3

Date and time of completion of the plating or other chemical process. Date and time of start of baking. Date and time of start of soak.

上一页第4页

你可能喜欢

热门文档

相关文档

  • AMS2759-5D中文版

    AMS2759-5D中文版_机械/仪表_工程科技_专业资料。马氏体不锈钢零件的热处理 1. 范围 本规范连同 AMS 2759 中提及的钢的热处理的一般要求一起, 构成了马氏体 ...

  • AMS5703D

    AMS 2759-9D-2009 钢制零件... 5页 5财富值 SAE AMS 5732J-2006 固溶热... 7页 10财富值 AMS H-6875A美国的军用热处... 29页 5财富值 AMS_5630G...

  • AMS2759

    AMS2759_交通运输_工程科技_专业资料。AEROSPACE MATERIAL SPECIFICATION AMS 2759... AMS2759-9D 5页 1下载券 AMS2759-1E 13页 1下载券 AMS2759-8A 13页 1...

  • AMS2759-3E

    AMS2759-3E_机械/仪表_工程科技_专业资料。美国国家标准今日推荐 ... AMS2759-2E AMS2759-5D AMS2759-8A AMS2759-9D AMS2759-9c1/2 相关文档...

  • AMS 2759-9

    AEROSPACE MATERIAL SPECIFICATION AMS 2759/9B Issued Revised NOV 1996 APR 2003... AMS 2759-7A 15页 1下载券 AMS 2759-9D-2009 钢制零... 5页 2下载券 ...

  • AMS2759-1E

    AMS2759-1E_机械/仪表_工程科技_专业资料。美国国家标准今日推荐 ... AMS2759-2E AMS2759-3E AMS2759-5D AMS2759-8A AMS2759-9D AMS2759-9c ...

  • AMS-H-6875A-V2

    环境 气态/燃烧废气 氩 3/ 氦 3/ 氢 3/ 氮 ...本文档零部件的任何参照被 AMS 2759 的相应要求取代...B 和 D 钢制热处理材料的硬度检测:最终热处理后的...

  • AMS2759-8A

    AMS2759-9D 5页 1下载券 AMS2759-5D 11页 1下载券 AMS2759-9c 5页 1下载券 AMS2759-5D中文版 8页 2下载券 AMS2759-3E 15页 1下载券 喜欢此文档的...

  • AMS2759-11

    AMS2759-11_机械/仪表_工程科技_专业资料。美国国家标准今日推荐 ... AMS2759-9D 5页 1下载券 AMS2759_2F 暂无评价 13页 1下载券 AMS2759-5D...

  • AMS 2759宇航材料规范

    2 AMS 2759/3C 3.3.1 果热处 ℉(774 热处理环境: 零件必须在空气中或保护气氛中热处理, 可接受的保护气氛包括氩、 氦、氢中性盐和真空。氮和氮氢混和物...