 导航当前位置: 文档下载 > 所有分类 > 工程科技 > 机械/仪表 > AMS 2759-9D-2009 钢制零件的除氢
侵权投诉

AMS 2759-9D-2009 钢制零件的除氢

原文

3.3.3.5 Soaking Interruptions 3.3.3.5.1

If the delay time (3.3.3.1) is less than 2 hours, soaking may be interrupted for the purpose of adding or

removing parts. If the delay time (3.3.3.1) is 2 hours or more, parts shall be soaked for at least one hour before any such interruption.

3.3.3.5.2 If the temperature indicated by the control instrument drops more than 25 °F (14 °C) below the set

temperature, the time during which the indicated temperature was below that temperature shall not be considered part of the soaking time of any parts in the furnace.

TABLE 1 - MINIMUM BAKE SOAK TIME (HOURS) AT 375 °F (191 °C)

Steel/Part

(9)

Description

AISI 1095

Specified (8)

Platings Treatments

Temper, Minimum

Cd

Strength (2)(3)(4)

& Ni

or Minimum

Cd-Ti (1)

Hardness 180 ksi (1241 MPa)

(5)

or 40 HRC

AF1410,

HP 9Ni-4Co-0.3C, All AerMet 100 Other High

Strength Carbon, (6)

or 46 HRC Low-Alloy,

Tool Steel

Lower Strength Carbon, Low- 180 ksi (1241 MPa)

(5) (7)

Alloy, or 40 HRC Tool Steel High Strength

Martensitic

(6)

or 46 HRC Stainless other

than 440C

Lower Strength

Martensitic (7)

or 40 HRC

Stainless 17-7PH®

15-7PH®

H950, RH950 17-4PH®

CUSTOM 455® & 465®

H950, H1000 23 23 8 23 8 8 3 8 23 3 NA

PH13-8 Mo® Stainless

NOTES:

NA - Not applicable (1) Or equivalent

(2) Includes electroless nickel, unless age hardened within four hours of plating (3) Chemical Processing: Etching, Stripping, Pickling, Chemical Milling

(4) Etch Inspection to detect abusive grinding/machining or the presence of carburizing - Baking is required after etch inspection when

hydrochloric or other reducing acid is used (e.g., AMS2649, Type 2 hydrochloric acid desmut). (5) Or higher, but having minimum less than 220 ksi (1517 MPa) or 46 HRC (6) Or higher specified minimum hardness

(7) Threaded fasteners - minimum 150 ksi (1034 MPa) and higher or 34 HRC or equivalent but minimum less than 180 ksi (1241 MPa)

or 40 HRC or equivalent - three hours for all processes

(8) For platings not listed, use baking time shown for cadmium.

(9) ® Custom 455 and Custom 465 are registered trade names of Carpenter Technology Corp.

17-7PH, 15-5PH, 15-7PH, PH13-8 Mo, and 17-4PH are registered trademarks of AK Steel (Armco).

上一页第3页

你可能喜欢

热门文档

相关文档

  • AMS2759-5D中文版

    AMS2759-5D中文版_机械/仪表_工程科技_专业资料。马氏体不锈钢零件的热处理 1. 范围 本规范连同 AMS 2759 中提及的钢的热处理的一般要求一起, 构成了马氏体 ...

  • AMS5703D

    AMS 2759-9D-2009 钢制零件... 5页 5财富值 SAE AMS 5732J-2006 固溶热... 7页 10财富值 AMS H-6875A美国的军用热处... 29页 5财富值 AMS_5630G...

  • AMS2759

    AMS2759_交通运输_工程科技_专业资料。AEROSPACE MATERIAL SPECIFICATION AMS 2759... AMS2759-9D 5页 1下载券 AMS2759-1E 13页 1下载券 AMS2759-8A 13页 1...

  • AMS2759-3E

    AMS2759-3E_机械/仪表_工程科技_专业资料。美国国家标准今日推荐 ... AMS2759-2E AMS2759-5D AMS2759-8A AMS2759-9D AMS2759-9c1/2 相关文档...

  • AMS 2759-9

    AEROSPACE MATERIAL SPECIFICATION AMS 2759/9B Issued Revised NOV 1996 APR 2003... AMS 2759-7A 15页 1下载券 AMS 2759-9D-2009 钢制零... 5页 2下载券 ...

  • AMS2759-1E

    AMS2759-1E_机械/仪表_工程科技_专业资料。美国国家标准今日推荐 ... AMS2759-2E AMS2759-3E AMS2759-5D AMS2759-8A AMS2759-9D AMS2759-9c ...

  • AMS-H-6875A-V2

    环境 气态/燃烧废气 氩 3/ 氦 3/ 氢 3/ 氮 ...本文档零部件的任何参照被 AMS 2759 的相应要求取代...B 和 D 钢制热处理材料的硬度检测:最终热处理后的...

  • AMS2759-8A

    AMS2759-9D 5页 1下载券 AMS2759-5D 11页 1下载券 AMS2759-9c 5页 1下载券 AMS2759-5D中文版 8页 2下载券 AMS2759-3E 15页 1下载券 喜欢此文档的...

  • AMS2759-11

    AMS2759-11_机械/仪表_工程科技_专业资料。美国国家标准今日推荐 ... AMS2759-9D 5页 1下载券 AMS2759_2F 暂无评价 13页 1下载券 AMS2759-5D...

  • AMS 2759宇航材料规范

    2 AMS 2759/3C 3.3.1 果热处 ℉(774 热处理环境: 零件必须在空气中或保护气氛中热处理, 可接受的保护气氛包括氩、 氦、氢中性盐和真空。氮和氮氢混和物...