ADVANCED WIRE BONDING-BONDING ON COPPER

copper wire introduction

Figure 3c. Cu bond pad after die attached curing

(snap cured). 3.3 Plasma Cleaning

Plasma cleaning prior to wire bonding would help to ensure copper bond pad cleanliness by removing the copper oxide. However, it is a known fact that without the appropriate set up, plasma cleaning could do more harm than good. In this evaluation, the wire bond is carried out without plasma cleaning.

4. Wire Bonding

The wire bonding was carried out on the ASM Wire Bonder AB339 Eagle. Both gold and copper wires were used. Figures 4a and 4b show the gold wire and copper wire ball bond on the copper die. Figure 4c shows a SEM picture of the copper ball bond.

Figure4a. Au wire ball bond on Cu bond pad

Figure 4b. Cu wire ball bond on Cu bond pad

Figure 4c. SEM picture of Cu ball bond

- 3 -

4.1 Influence of the Bonding Stage Temperature

It is well known that copper oxidize readily when expose to high temperature. Hence, the following experiment is carried out to study the influence of the bonding stage temperature. A ball bond was bonded onto the copper die at an interval of 15 seconds. The bonding continued until non-stick of the ball bond occurred. The non-stick of ball bond is an indication of oxidation of the copper bond pad. This is related to the rate of oxidation. This same evaluation is carried out at different bonding temperature ranging from 145 C to 170 C. Figure 5a shows the relationship between the stage temperature and oxidation rate. For a stage temperature of 145 C, it has been observed that there is no non-stick at even after 6 minutes of exposure. Figure 5b shows the ball shear test carried on this unit. It could be seen that there is no decrease in the ball shear strength after 6 minutes.

ADVANCED WIRE BONDING-BONDING ON COPPER

Figure 5a. Relationship between the stage temperature and oxidation rate (non-stick of ball

bond)

ADVANCED WIRE BONDING-BONDING ON COPPER

Figure 5b. Relationship between ball shear and bond

stage exposure time at 145 C

5. Analysis of Copper Bond Pad Surface with OIM

ADVANCED WIRE BONDING-BONDING ON COPPER

It

ADVANCED WIRE BONDING-BONDING ON COPPER

has

ADVANCED WIRE BONDING-BONDING ON COPPER

been

ADVANCED WIRE BONDING-BONDING ON COPPER

observed that within the same lot of wafers, some are bondable even without plasma cleaning whereas some are not. This is most likely due to the oxidation of copper and pad surface. One of the advanced techniques for detecting the initial stages of oxidation

上一页第3页

你可能喜欢

热门文档

相关文档

  • Copper_Wire_Bonding_Training

    Copper Wire Bonding Training 铜线焊线培训 Prepared by: Ning wy Shenzhen STS Microeletronics Copper Wire Bonding Content of Presentation 内容介绍 Advantages优点...

  • Developments in Copper Wire Bonding

    Drivers for Cu Wire Bonding ? ? ? ? Cost, cost and cost Gold price continues to increase: $1,515.17/oz on 2011-05-04 Copper: $4.15/lb Early...

  • Fine Pitch Copper Wire Bonding Process and Material...

    Wire Bonding Optimizatio... 6页 20财富值 Gold Wire Bonding On Low... ...The study has shown the utilization of advanced wire bonder copper capability...

  • Wire bonding workmanship standard

    wire bonding工艺文件 12页 2下载券 Copper Wire Bonding 5页 7下载券 喜欢...REJECT if no gold ball and or wire observed on bond pad and substrate ...

  • Heraeus Copper Wire Presentation

    Market Review Challenges in Copper Wire bonding Heraeus Copper Wire Portfolio ...? Soft wire characteristics enable: ? Bonding on challenging pad structure. ...

  • Reliability of copper wire bonding in humidity envi...

    In present paper, copper wire bonding on palladium finish and gold finish was studied to investigate the interface degradation during uHAST comparing with ...

  • Wire Bonding process

    Hardening: Advanced deformation, diffusion initiate Saturation: Bond finished ... Fine Pitch Copper Wire... 8页 免费 Wire Bonding Summary 25页 免费 ...

  • Chapter7_Reliability_Advanced_bonding_interconnecti...

    Development of Copper Wi... 6页 20财富值 ... Advanced Bonding Interconnection Technology (Chapter...Bonding styles – Al wire bonding on Cu pad, ...

  • Cu wire bonding

    (<=1.3mil) ~ 26% of the TAM Bonding Wire 18 Copper Wire Market Trend...Materials Characteristics of Soft Copper Wires Designed for Advanced Applications...

  • ...and Feasibility of Copper Wire bonding for Non-h...

    Many studies have been done on copper wire bonding for equipment capability,...Also, an advanced tip surface finishing in order to executes better gripping...

站点地图 | 文档上传 | 侵权投诉 | 手机版
本站所有资源均来自互联网,本站只负责收集和整理,均不承担任何法律责任,如有侵权等其它行为请联系我们.
文档下载 Copyright 2013 doc.guandang.net All Rights Reserved.  -  email