GONG Wei-huai, et al/Trans. Nonferrous Met. Soc. China 21(2011) 2044 2048 2045
potentiodynamic polarization. The results indicate that
the laser-welded NiTi alloy is less susceptible to pitting and crevice corrosion than the base metal.
However, previous studies on the welding of TiNi SMA are mainly to TiNi wire or thick TiNi sheet above 1.5 mm in thickness. But the welding of ultra-thin TiNi SMA sheet has bright prospect in the field of medical device, aviation and space-flight. The authors of this work have realized butt welding of 0.2 mm-thick TiNi SMA sheet using impulse micro laser [16]. The aim of this work is to investigate the microstructure and properties of 0.2 mm-thick TiNi SMA sheet welded joint.
2 Experimental
0.3 mm-thick TiNi SMA (Ti49.4Ni50.6 in mole fraction, %) was used as the base metal in this investigation. The sheets were produced by coldrolling with a thickness reduction of about 22%. In order to remove the surface layer of oxide produced during the coldrolling process, the TiNi sheets were degreased with propanone and soaked for 15 min in the mixture solution of hydrofluoric acid and nitric acid, and then washed with clear water and weathered. After these treatments, the width of the sheets was 0.2 mm. The dimensions of the welding specimens were 0.2 mm×40 mm×60 mm.
The welding process was carried out using a Nd:YAG laser source(SL 80, made in Italia, average power is 80 W). In order to protect the welding zone, a special clamping fixture was built to protect both frontal surface and back surface of the welded joint. After preliminary experiment, nine groups of experiment parameters shown in Table 1 were carried out. For all experiments, the spot diameter, welding rate and argon flow rate were fixed at 0.3 mm, 0.3 mm/s and 5 L/min, respectively.
After welding, tensile samples of every group of welding parameters were made by spark cutting and
Table 1 Welding parameters for laser micro welding of 0.2 mm-thick TiNi SMA
Weld Power Impulse Impulse sample No. percent/% width/ms frequency/Hz 1 15 1.5 4 2 15 1.9 5.5 3 15 2.3 7 4 18 1.5 5.5 5 18 1.9 7
6 18 2.3 4
7 21 1.5 7
8 21 1.9 4
9 21 2.3 5.5 tensile properties of welded joint were tested on a tensile testing machine (INSTRON 5540). Scanning fracture morphology of tensile sample was observed with electronic microscope (Quanta 200). Metallographic specimen was made along cross direction of the welded joint and etched with mixture acid solution of HF and HNO3. The microstructure and element distribution were studied with metallographic microscope (4XB-TV).
The welded joint and base metal were annealed at 500 °C in vacuum for 1 h, and the SMA of annealed welded joint and annealed base metal was tested by DSC measurements which were performed using a SEIKO in temperatures ranging from 60 to 200 °C under a controlled cooling and heating rate of 10 °C/min.
3 Results and analysis
3.1 Tensile properties and fracture morphology
Tensile strength values of the nine groups of experiment parameters are shown in Table 2. When power percent is 21%, pulse frequency is 4 Hz, and pulse width is 1.9 ms (welded sample No. 9), the welded joint has the best tensile strength of 683 MPa, which is 97% of the strength of base metal.
Table 2 Tensile strength of laser micro welded joint of 0.2 mm-thick TiNi SMA with different welding parameters
Sample No.
Tensile strength/MPa
1 522 2 265 3 613 4 397 5 450 6 353 7 445 8 683 9 623 Base metal
705
Figure 1 shows the stress—strain curve obtained from the welded joint of weld sample No.9. The curve
indicates that high tensile strength of the welded joint could be gained by laser micro welding. The fracture
strain of the welded joint is 5.8% which achieves 95% of that of the base metal. It is of interest to note that the stress—strain curve is smooth and continuous at all the strain rates.
All the nine groups of welded samples failed at the welded seam edge near HAZ among which an example is
shown in Fig. 2. The welded joints show basically
similar features on the fracture surfaces, typical SEM
micrographs of the fracture surface of the welded sample
and banse metal can be seen from Fig. 3. Cup-like
黑龙江哈尔滨150001)(2.南吕航空人学,江西南昌330063) 摘要:采用微型脉冲激光对0.2mm厚的薄片状TiNi形状记忆合金/不锈钢异种材料进行对接焊,研究了接头的微观 组织...
利用光学显微镜,扫描电镜,微区XRD等分析测试手段,研究了TiNi形状记忆合金丝激光焊接头的微观组织特点。为研究接头的力学性能和形状记忆效应,对其进行拉伸和弯曲试验。...
TiNi形状记忆合金与不锈钢激光钎焊接头界面组织特征_专业资料。通过扫描电子显微镜、能谱仪及X射线衍射技术分析TiNi形状记忆合金与1Cr18Ni9Ti不锈钢激光钎焊接头界面反应...
TC4钛合金激光焊接接头组... 4页 免费 TiNi形状记忆合金片激光... 5页 1...形貌, 研究了接头的微观组织和性能, 分析了晶间析 出相物对接头性能的影响。...
预置填充稀土激光焊接对TiNi形状记忆合金微观组织及成分的影响_专业资料。采用Nd—YAG连续激光器对Ti—Ni50.9at%形状记忆合金进行焊缝预置填充材料激光焊接,预置填充...
能焊和激光钎焊焊接 TN 形状记忆合金与不锈钢异质接头 , ii 研究 了接头 的力...口形貌和微观组织.结果表明 : 采用微束等离子 弧焊和储能焊 , 焊接接头极脆 ...
作者在 TiNi 形状记忆合金激光 对接接头的焊缝中预置填充混合稀土元素,改善了激 光焊缝组织性能,对记忆合金的激光焊接领域拓展有 更好的前景。 1 1.1 实 验 ...
试验研究了TiNiNb宽滞后形状记忆合金Nd:YAG激光焊接的组织与性能。通过光学显微镜...β-Nb在TiNi基体相晶界和晶内分布不均匀;接头各区域的显微硬度均高于母材;室温...
喜欢此文档的还喜欢 TiNi形状记忆合金片激光微... 5页 2财富值... 微观组织演变对ZK60合金搅拌摩擦焊接接头的力学性能的影响(英文) 隐藏>> ...
No.10 October 2008 预置填充稀土激光焊接对 TiNi 形状记忆 合金功能性的影响...激光焊接接头的组织与原母材组织有明显变化,在瞬 时高能量密度的激光源作用下,...
热门文档