10524Ind.Eng.Chem.Res.,Vol.48,No.23,

2009
Table1.ResultsofScoroditeCrystallizationatDifferentTemperaturestemp(°C)507095170
residencetime3days5h3h5h
%w/wAs31.0532.2332.5633.13
Fe21.7723.0222.9024.21
TCLPlixiviationofAs(mg/L)
40010010021

averagesizeofparticle(µm)
10.021.018.19.8
and95°Candcrystallizationoccurredinanautoclave,usingthesameprocedureat170°Candthepressureat130psi.For170°C,aninitialconcentrationof8%Asand6%Fewasused.TheautoclavewasfromParrInstrumentCo.,ModelBenchTopReactors4520,madeoftitanium,with1-Lcapacityandtemperaturecontrolfrom0to800°C.ResultsandDiscussion
ScoroditeCrystallizationStudy.AlltheexperimentswereconductedwithamolarratioofFe/Ase1andanagitationvelocityof300-400rpm.Sloweragitationspermitthecrystalstosettleandfasteragitationscausecrystaldamage.TheexperimentalresultsareshowninTable1.Table1summarizestheresultsofthetestsforobtainingscoroditeforallworkingtemperatures.The nalpHofthesolutionobtainedafterthecrystallizationwas1foralltheexperimentscarriedout.
EffectofTemperatureandTCLP.Thesystematatmo-sphericpressurewasstudiedatthreedifferenttemperatures:50,70,and95°C.Accordingtotheexperimentalresults,temper-atureandresidencetimepresentaproportionallyinverserelationship,ascanbeseeninTable1.OurresultsareinagoodagreementwiththoseofLeBerre12andSinghania.6Thecoloringofthecrystalsalsovariedwithtemperature.At50and
70°C,thecrystalshaveanivorycolor,andat95°Ctheyarebeige-green.TemperaturealsoplaysaveryimportantroleonscoroditestabilityagainsttheTCLPtest.AsTable1shows,thehigherthetemperature,themorestablethescoroditethatisobtained.Nomajordifferenceinthesolubilityofthecrystalisnotedat70and95°C.
ScoroditeProducedinanAutoclaveandTCLP.Thecrystalsobtainedinthisexperimenthaveapalegreencolor,ratherdifferentfromthecrystalssynthesizedatatmosphericpressure.ThesecrystalsarealsomorestableaccordingtotheTCLPtest([As])21mg/L),comparedtotheexperimentscarriedoutat95and70°C([As])100mg/L;seeTable1).Thecrystalsproducedintheautoclavearethemoststable,andwillthereforebeusedasseedinfutureworks.ItisworthnotingthattheTLCPtestforthissolidiswelloverthepermittedlimitofarsenicsolubility(5mg/L),perhapsbecausetheformationofFe2(HAsO4)3·xH2O,calledtypeonephasebyUgarte,1formsatmolarratioFe/As)1andtemperaturesabove150°C.ParticleSize.TheaveragesizeofcrystalswasdeterminedfordifferenttemperaturesasshowninTable1.Nocleareffectofcrystallizationtemperaturewasobservedontheaveragesizebecausecrystallizationswerereachedwithoutcontrolofthedegreeofoversaturation.Consequently,thesizesobtainedweresmallandsusceptibletoagglomeration.
Theresultsshowthatthecrystalsproducedintheautoclavearethesmallest,likelyduetoeithermechanicalagitationorlessagglomerationofcrystalsbecauseoftemperature.Neverthe-less,thissizeisappropriateforuseasseed.6
DiffractogramAnalysis.Figure1showsdiffractogramsofthesolidresiduesexperimentallyobtained.Theblacklinerepresentsthescoroditesynthesizedintheexperiment.Thered
Figure1.Diffractogramsofthescoroditesynthesizedat(a)50,(b)70,(c)95,and(d)170°C.
热门文档