°Cwasrequired(ideally160°C)toensuregoodcrystallinity.Scoroditeissolubleinwaterinthearsenicrangeof0.1-3.6mg/L.6,8,9

Inamorerecentwork,DutrizacandJambor10carriedoutscoroditecrystallizationusinganautoclaveinatemperaturerangeof150-175°CbymixingFe(SO4)1.5,H2SO4,andAs2O5,showingthefeasibilityofproducingscoroditeattemperaturesabove150°C.

SwashandMonhemius11foundthatamorphousferricarsen-ateshavehighersolubilitythancrystallinescorodite,byap-proximately2ordersofmagnitude.TheyalsoobservedthatferricarsenatesbegintoprecipitateatpHvaluesbetween1and2,whiletheformationofcalciumarsenatesbeginsatpHbetween3and4.

LeBerreetal.12studiedthetransformationofferricarsenateofpoorcrystallinityandcrystallinescorodite,workingatdifferenttemperatures(40,60,80°C).Asaresult,theyfoundthatthelengthofinductionistotallydependentontemperatureandpH.WhilepHremainsat2,theinductionperiodisaround9hat80°C,increasesto40hat60°C,andincreasesto240hat40°C.Ontheotherhand,iftemperatureismaintainedat80°CandpHisincreasedfrom2to4,theinductionperiodincreasesbyalmost10times.Besides,acolorchangeoftheprecipitateisveri edasafunctionoftime,indicatingresidencetimedependence.Diffractogramsofeachtestwerecomparedtothecrystallinescoroditepattern, ndingthecharacteristicpeaksforthe rsttimeat10h,thusprovingthatthelongertheresidencetime,thehigherthecrystallinity.

Fujitaetal.13studiedtheeffectsofreactiontemperature(95,70,50°C)andtheoxidizingagent(air,pureoxygengas)tooptimizescoroditeformationinapracticalprocess.Theirresultsindicatethatcontrolledsynthesisat70°Cachievedsuf cientlystablescoroditeparticlesandthatairoxidationproducedscorodite,evenat50°C.The nalconcentrationofarsenicat70°Cwassameasthatat95°C.Areactiontemperatureof50°Cwasnotsuf cient.Theresultsindicatedthatvery necrystalsformedat50°Cagglomeratetoproducelargerparticles,whileathighertemperatures,thesmallerparticlesaremorecrystallineanddiscrete.

Thepresentstudyhastheobjectiveofdesigningaprocessforextractionofarsenicfromaresidualliquidwithconcentra-tionstoindustriallevels.Thearsenicwasextractedthroughcrystallizationofferricarsenate(scorodite,FeAsO4·2H2O)attemperaturesoflessthan100°C.

Themethodologyemployedwastouseexperimentalstudiesofthecrystallization,reactionkinetics,andphaseequilibriumofthesystemAs-Fe-H2Oat(50and70)°C,14whichprovidedtheoperationalconditionsoftheprocess.

Theeffectoftemperatureinscoroditecrystallizationandthestabilityofcrystalsasresidue(TCLPtest15)werestudied.Thecrystalsobtainedwerechemicallyanalyzed.

Withtheaforementionedinformation,aprocesswassimulatedusingMETSIMsoftwarethatallowedforreducingthenumberofexperimentsinthelaboratoryandprojectingexperimentalresultstoanindustrialprocess.METSIM16softwarecomputesmassandenergybalancesinasteadyordynamicstate,includingprocesscontrolandchemicalreactions,alongwithagreatnumberofunitaryoperations.AlgorithmscanbeincorporatedusingAPL,aconcisecomputerprogramminglanguage.

A ctitiousfeedingsolutionwasusedfordesigningtheprocess.Thepointthatrepresentsthefeedingsolutionislocatedinthephasediagramanddeterminesthenecessaryprocessestoenterthecrystallization eldandobtainscorodite.

Ind.Eng.Chem.Res.,Vol.48,No.23,200910523

Tosimulatetheprocess,threecaseswereevaluatedwithdifferent ows.Yields,equipmentsize,andrequiredenergywerestudied.Aswell,theconversionvariablesofthereactionforformingscoroditeandtheFe/Asmolarratioincrystallizationwerestudied.

ExperimentalProcedure

Materials.Theanalyticalgradereagentsusedwerethefollowing:arsenicpentoxidehydrate(As2O5·3H2O),SigmaAldrich,98%;sodiumhydroxide(NaOH),Merck,99%;ferric

sulfatepentahydrate(Fe2(SO4)3·5H2O),Riedel-DeHae

¨n,21-23%Fe;andultrapurewater(conductivitye0.05µS/cm)obtainedbypassingdistilledwaterthroughaMilliporeultrapuredevice.FerrichydroxidewaspreparedinthelaboratoryjustbeforeeachexperimentbythereactionofNaOHandFe2(SO4)3·5H2O.ThiswasdonebecauseactiveFe(OH)3isrequiredandthecommercialvarietydoesnotmeetthisrequirement.

EquipmentandExperimentalProcedure.Crystallizationswerecarriedoutina250cm3Pyrexcrystallizerwithaheatingjacket.ThecrystallizerincludedathermoregulatedLaudaRM-Bbath,witha6-Lcapacityandtemperaturecontrolfrom-20to100°C(0.1°C.Forscoroditecrystallization,Fe(OH)3(s),As2O5·3H2O(s),andwaterweremixed.Thereactiontempera-tureswere50,70,and95°C.Thesetemperatureswerechosenbasedonequilibriumphasediagramsreportedinapreviousstudy.14Aswell,itwasdesiredtoobtainscoroditecrystallizationattemperaturesoflessthan100°C.At95°C,thephasediagramisassumedtobesimilartothatobtainedat70°C.Thereagentconcentrationsforscoroditecrystallizationweredeterminedaccordingtotheproportionsgivenbythephasediagrams14inthecrystallizationzone.Attemperaturesof50,70,and95°C,aninitialconcentrationof9.7%Asand7%Fewasused,inthelineofthemaximumyieldofthescoroditecrystallization eld(point1,Figure4).Thesolutionsreactedinthecrystallizerunderwell-controlledheatingwhilebeingmagneticallyagitated(300-400rpm).Theresidencetimebeganoncethetemperaturewasreachedandthereactivesweremixeduntilprecipitatingscoroditewasachieved.

Tostopthereaction,thesuspensionswerevacuum ltered,thepHoftheliquidswasmeasured,andthesolidwaswashedwithdistilledwateranddriedatroomtemperatureuntilreachingaconstantweight.Thesolidsandliquidsobtainedwereanalyzedbyatomicabsorptionspectrometry(AA),usingaVarianModelSpectrAA220instrument.Aswell,thesolidswerecharacterizedbyX-raydiffractionusingaSiemensD5000X-raydiffracto-meterandweresubmittedtoaTCLPtestandsizedistributionanalysis.Theparticlesizedistributionwasdeterminedusinganautomaticanalyzerofcentrifugalparticlesizedistribution,HORIBACAPA-300.

TheTLCPtestwascarriedoutonthecrystalsinordertodeterminethestabilityofsaltsandtoevaluateiftheywerepotentiallyinterestingasalternativewastematerialsinindustrialprocesses.TheTCLPtestestablishedstandardsintermsofconcentrationlimits.Thisprocedureconsistedofleachingasolidsamplefor18hinaweaksolutionofaceticacidinaliquid/solidproportionof20:1,withagitationof30rpmandatemperatureof22°C.Oncethetestwascompleted,the lteredsolutionwasanalyzed,consideringastablesolidwhenarsenicdidnotexceed5mg/L.ThesolutionsobtainedfromtheTCLPtestwerecharacterizedbyatomicabsorptionspectrometry.(Note:Forverylowarsenicconcentration,thegenerationofhydridesisnecessary.)

Withtheobjectiveofknowingtheeffectoftemperatureonproductquality,crystallizationtestswerecarriedoutat50,70,