Fig. 3 Optical microstructure of original NiTi SMA tube

2.3 ECAE process

The assembled NiTi SMA tube samples were placed into the ECAE die and then they were put into the Instron 5500R universal testing machine, where the assembled SMA NiTi tube samples were heated to 500 °C. Subsequently, the pressing punch moved down at the speed of 1 mm/s. Consequently, the assembled SMA

NiTi tube samples were forced to go across the channel

of the die and thus the ECAE process was finished.

2.4 Compression test

The NiTi SMA samples with the diameter of 4 mm and the height of 6 mm were prepared from the NiTi SMA bar whose state was identical to the NiTi SMA tube for ECAE and were used for compression test in order to obtain the constitutive model of the NiTi SMA. In the same manner, the steel samples with the diameter of 4 mm and the height of 6 mm were prepared from the low carbon steel used for the steel can and the steel core

for ECAE and were used for compression test in order to

Fig. 4 Stress—strain curves of NiTi SMA at 500 °C obtain the involved constitutive model. The compression

experiments were carried out on the Instron 5500R

3.2 Finite element model universal testing machine at the strain rates ranging from

DEFORM3D finite element code was used to 0.001 s 1 to 1 s 1 and at 500 °C.

simulate ECAE of NiTi shape memory alloy tube. Figure

7 indicates the finite element model of ECAE of NiTi 2.5 Microstructural observation

SMA tube. It can be seen from Fig. 7 that the boundary The microstructures of the compressed NiTi SMA

conditions are very complicated and there exist multiple samples as well as the NiTi SMA tubes before ECAE and

after ECAE were observed by means of optical coupled boundary conditions, such as between NiTi tube

and steel core, between NiTi tube and steel can, between microscopy. All the specimens for optical microscopy

NiTi plug and steel can, between NiTi plug and NiTi tube, were etched in a solution of 10% HF + 40% HNO3 +

between NiTi plug and steel core, between steel core and 50% H2O.

steel can, between steel can and die, between steel can

3 Finite element simulation of ECAE of NiTi and punch and between NiTi plug and punch. According

to the ECAE process parameters, the pressing speed of SMA tube

the punch is selected as 1 mm/s, and the pressing stroke

3.1 Constitutive model of the punch is determined as 20 mm during the finite

Establishing the appropriate constitutive model of element simulation.

NiTi SMA plays a significant role in simulating ECAE

of the NiTi SMA tube. Figure 4 demonstrates the stress—strain curves of NiTi SMA at 500 °C and the strain rates of 0.001, 0.01, 0.1 and 1 s 1, respectively. It can be seen from Fig. 4 that the true stress of NiTi SMA increases with increasing the strain rate, which indicates that NiTi SMA is sensitive to the strain rates and thus belongs to rigid-viscoplastic materials at 500 °C. Figure 5 shows the microstructures of the involved compressed samples at different strain rates, which reveal that NiTi SMA is obviously characterized by dynamic recovery at all the strain rates instead of dynamic recrystallization. Therefore, ECAE of NiTi SMA tube was carried out at 500 °C. The constitutive model of NiTi SMA in Fig. 4 shall be used as the material model in subsequent finite element simulation of ECAE of NiTi SMA tube. The true stress—strain curves of the low carbon steel for the steel can and the steel core at 500 °C are illustrated in Fig. 6 and are used as the material model of the steel can and the steel core during ECAE of NiTi SMA tube. Therefore, multiple constitutive models including NiTi SMA tube, NiTi plug, steel can and steel core are applied during ECAE of NiTi SMA tube.

镍钛形状记忆合金管的等通道转角挤压_英文_江树勇

镍钛形状记忆合金管的等通道转角挤压_英文_江树勇

镍钛形状记忆合金管的等通道转角挤压_英文_江树勇

镍钛形状记忆合金管的等通道转角挤压_英文_江树勇

上一页第3页

你可能喜欢

热门文档

相关文档

站点地图 | 文档上传 | 侵权投诉 | 手机版
本站所有资源均来自互联网,本站只负责收集和整理,均不承担任何法律责任,如有侵权等其它行为请联系我们.
文档下载 Copyright 2013 doc.guandang.net All Rights Reserved.  -  email