2.2.14 Cr-Mo-V-Ti-B steel

96 2.2 Low alloy steels

2.2.14 Cr-Mo-V-Ti-B steel

2.2.14.1 Introduction

Cr-Mo-V-Ti-B steel (Durehete 1055) is used in fasteners for turbines and process plants and as boiler support rods. It is part of the Durehete series of creep resisting steels and was developed originally in the 1950’s in response to the increases in operating temperatures in steam power plants. The earlier alloy Durehete 900 was a CrMo base. Improved high temperature properties were obtained by the addition of V resulting in the 1%Cr, 1%Mo, 0.75%V steel, Durehete 950. Further improvements were obtained by adjusting the carbon and vanadium to near stoichiometric levels maximizing the elevated temperature strength to give the alloy Durehete 1050. However the high strength of this material was coupled with poor ductility which resulted in grain boundary cracking after relatively short exposures at 550 - 565 °C. Durehete 1055 was the result of further development to improve the ductility. Additions of Ti and B were made resulting in a finer austenite grain size. Further enhancement of the ductility, and hence a decrease in the susceptibility to grain boundary cracking, has been produced by control of residual levels principally phosphorus, arsenic, tin, antimony and copper.

Durehete 1055 is suitable for use at temperatures up to 570 °C (approximately 1055 °F). 2.2.14.2 Material standard, chemical composition and mechanical property requirements

Table 66. Chemical requirements for Cr-Mo-V-Ti-B steel, Durehete 1055; EN 10269:1999

Chemical composition [wt%] Stan-Designation

dard 20CrMoVTiB 0.17 ≤ 0.35 ≤ 0.90 0.90 ≤ 0.0150.0010.60 0.07 ≤ ≤ ≤ ≤

EN 0.23 0.40 0.75 0.0200.0201.20 1.10 0.20 0.0800.0100.80 0.15 0.20 4-10

The material is usually supplied in the oil or water quenched and tempered condition. The recommended austenitizing temperature range is 970 - 990 °C with tempering in the range 680 - 720 °C.

Table 67. Room temperature mechanical property requirements for Cr-Mo-V-Ti-B steel, Durehete 1055; EN 10269:1999 Stan-Std. Heat Diameter d Rp0.2 Rm A Z Cv(RT)

Designation

dard No. treat [mm] [MPa] [MPa] [%] [%] [J]

820 ≥ ≥ ≥ ≥

≤100

1000 15 660 50 40 102620CrMoVTiB

EN Q+T

9:99 4-10 820 ≥ ≥ ≥ ≥

100 < d ≤ 160

1000 15 660 50 27

Table 68. Minimum 0.2% proof strength values at elevated temperatures for Cr-Mo-V-Ti-B steel, Durehete 1055; EN 10269:1999

Minimum 0.2% proof strength, Rp0.2 [Nmm] at a

Heat Diameter Stan-Designation temperature [°C] of treat [mm] dard

50

100150200250300350Q+T ≤160

4-10

+ values calculated by linear interpolation EN

642+624603595581573559

Landolt-Börnstein New Series VIII/2B

第1页

你可能喜欢

热门文档

相关文档

  • DIN EN 970 EN 1997_03

    Analysis of aluminium ... 暂无评价 36页 免费 2.2.14 Cr-Mo-V-Ti-B st... 暂无评价 4页 1下载券2014 Baidu 使用百度前必读 文库协议...

  • DIN EN 970 EN 1997_03

    Analysis of aluminium ... 暂无评价 36页 免费 2.2.14 Cr-Mo-V-Ti-B st... 暂无评价 4页 1下载券2014 Baidu 使用百度前必读 文库协议...

站点地图 | 文档上传 | 侵权投诉 | 手机版
本站所有资源均来自互联网,本站只负责收集和整理,均不承担任何法律责任,如有侵权等其它行为请联系我们.
文档下载 Copyright 2013 doc.guandang.net All Rights Reserved.  -  email