Comparison Of Failure Criteria For Jointed Rock Masses

Comparison Of Failure Criteria For Jointed Rock Masses 节理岩体破坏准则比较

Table 3 Hoek and Brown paramters for different

rocks

Hoek andRock TypeRMR

Brown

parametersii

Intact Kota

sandstone89151

Sandstone57151

Gypsum

Plaster2071

Numerical analysis of a powerhouse cavern inthe state of Himachal Pradesh India, namelyNathpa Jhakri Cavern is then taken up. Thepowerhouse cavern has dimensions 216 m × 20 m× 49 m (length × width × height) at a depth of262.5 m below the ground level. The rock massaround the cavern is mainly quartz mica schistwith joints and discontinuities [Bhasin, (1996) andSitharam & MadhaviLatha (2002)]. The measuredin-situ stresses are 4.73 and 6.34 MPa in E-W andN-S and directions respectively and 5.89 MPa invertical direction. The geometry of the cavernalong with the excavation sequence and locationof extensometers is shown in Figure 2.

Comparison Of Failure Criteria For Jointed Rock Masses

Comparison Of Failure Criteria For Jointed Rock Masses

EL 1022 m

EL 996 m EL 975 m

Comparison Of Failure Criteria For Jointed Rock Masses

Figure 2. The rock mass at the site has one set of jointsinclined at 55° with joint frequency of 5 per meterdepth. The joint factor for the rock masscalculated using equation 9 is 22. The RMR value

for the rock mass estimated as per Bieniawski(1973) is 52.

In this paper, numerical analysis of the cavernis carried out using both the failure criteriaexplained. Properties of intact rock at Nathpa-Jhakri cavern are given in Table 4.

Table 4 Properties of intact rock for Nathpa-Jhakri powerhouse cavern

Uniaxial compressive strength (MPa)16Young's modulus (MPa)8591Angle of internal friction (degrees)22

i

Ramamurthy’s Bi2.5Hoek and Brown parameter mi2.03i3.The comparisons between the numericallyRESULTS AND DISCUSSION

predicted and the experimental stress-strainbehaviour of three rocks at different confiningpressures using different failure criteria are shownin Figures 3-5.

100

80

)

aMP60

s (estr soratvi40

De20

0.0

0.2

0.4

0.6

0.81.0

1.2

1.4

1.6

Axial strain (%)

Figure 3. Comparison of stress-strain curves

for intact Kota sandstoneIt can be observed that the predicted stress-strain curves closely follow the experimental dataat all lower and higher confining pressures for thecase of intact Kota sandstone.