JOURNALOFMATERIALSSCIENCELETTERS20,2001,333–335
EffectofagingonthehardnessandimpactpropertiesofHastelloyC-276
J.I.AKHTER,M.A.SHAIKH,M.AHMAD,M.IQBAL,K.A.SHOAIB,W.AHMAD
NuclearPhysicsDivision,PakistanInstituteofNuclearScienceandTechnology,Nilore,Islamabad,PakistanE-mail:pinstech@paknet2.ptc.pk;akhterji@usa.net
Nickelbasealloysconstituteanimportantclassofmaterials,whichareusedunderdemandingcondi-tionsofhighcorrosionresistanceandhightempera-turestrength.Awiderangeofthesealloysexistsduetotheabilityofnickelmatrixtoaccommodatelargeamountsofelements,suchaschromium,iron,copper,molybdenum,etc.,whileretainingessentiallyasinglephaseface-centered-cubicstructure[1].Ni-Cr-Mo-Walloys,namedasHastelloys,areknownfortheirgoodmechanicalandphysicalpropertiesandresistancetoawidevarietyofcorrosiveenvironments.Thealloyshavefoundwidespreaduseinchemical,aerospaceandnuclearindustrybecauseoftheseproperties.
HastelloyC-276hasbeenpreviouslystudiedduetoitsmanyapplications.Effectofagingtreatmentonthemicrostructureandcorrosionpropertiesofthisalloyhasbeeninvestigatedbyanumberofresearchers[2–5].Precipitationofintermetallicphases(µandP)andcarbideshasbeenreportedinmostofthesestud-ies.Theµphaseisknowntobehardandbrittle[5].Ontheotherhandthisalloyhasbeenconsideredtobenon-hardenablebyconventionalagingtreatment[6].Presentstudyhasbeencarriedouttoinvestigatetheeffectofagingtreatmentonthehardnessandimpactenergyofthematerial,asnodetailedresultsareavail-ableontheseaspects.Theresultswouldbecorrelatedwiththeprecipitatesproducedduetoheattreatment.HastelloyC-276wasreceivedintheformofasheethavingthickness3mm.ThecompositionofthealloyisgiveninTableI.Samplesweresolutiontreatedat1200 Cfor1handwaterquenched.Agingwascar-riedoutattwotemperatures650 Cand850 Cfortimevaryingupto240h.Specimenswereetchedinaso-lutionof10–12%.HClinethanolandthentheywereexaminedinscanningelectronmicroscope(SEM).El-ementalanalysiswasdoneusingX-rayenergydisper-sivemicroanalysissystem(EDS)attachedwithSEM.Precipitateswereextractedforanalysisusingcarbonreplicatechnique.Sampleswerepreparedforimpacttesting withsize3×10×55mm3andhavingnotchof45angle.Thesesamplesweretestedwith50Jhammer.Hardnessofthealloywasmeasuredinthreecon-ditions,i.e.as-received,solutiontreatedandagedbyRockwellhardnesstester(HRB).Hardnesswasfoundtoremainconstantforthesamplesagedat650 C.Itsvalueisthesameasthatofthesolutiontreatedsam-ples.Itsuggeststhatnohardeningphasesareproducedat650 Cforagingtimeupto240h.Accordingtothepreviouslyreported[2]time-temperature-precipitation
0261–8028
C2001KluwerAcademicPublishersdiagramoneofthehardeningphases,i.e.,µphaseisnot
formedat650 Cupto500hofaging.HoweverMmaybeproducedafterabout10hofaging.6CcarbidesInthepresentcasenoprecipitateshavebeenobservedbySEMexaminationinthesamplesagedat650 Cforagingperiodupto240h.Itmaybethatprecipitationofcarbidesmaytakemuchlongerthantheagingtimeperiodinthepresentcase.Roomtemperatureabsorbedenergiesofthesampleswereattemptedbyimpacttest-ingaftervariousagingtreatments.At650 C,nosamplecouldbebrokenshowingagainthathardeningwasnotproducedbyagingatthistemperature.
Hardnessofthesamplesagedat850 Cincreaseswithagingtimeupto96handthenremainsconstant.TheseresultsareplottedinFig.1.Thesemeasurementssuggestthatagingat850 Chardensthealloy.Thisob-servationiscontrarytothepreviouslyquotedstatement
TABLEIX-raymicroanalysis(wt.%)ofmatrixandprecipitates.Numberswithinthebracketsindicate±σ.KlinesforNi,Cr,Fe,Co,LlineforMo,andMlineforWwereusedElementMatrixPrecipitatesPreviousresultsNi54.49(0.37)25.45(0.75)28.0(2.4)Mo17.26(0.50)46.30(0.80)49.5(2.2)Cr16.25(0.30)11.77(0.42)11.0(0.4)Fe5.49(0.30)3.42(0.34)2.0(0.2)W4.62(0.37)11.38(0.53)7.5(2.6)Co
1.67(0.31)
1.68(0.38)

1.5(0.1)
Figure1Variationofhardnessandimpactenergyasafunctionoftem-perature.
333
Therefore, a systematic study on the corrosion ...2. Experimental The plate of Hastelloy C-276 is...Allen, The effect of grain boundary engineering ...
Properties Hardness and Impact Strength Tensile Data...HASTELLOY C-22 alloy HASTELLOY C-276 alloy ... Aged Sheet* Aging Temperature, °F (°C) No...
(8条) 1.Akhter J I;Shaikh M A Effect of Aging on the Hardness and Impact Properties of Hastelloy C-276[外 文期刊] 2001 2.吴嘉伟;董建新;曾燕萍...
alloy HASTELLOY C-276 alloy (N10276) HASTELLOY ....06C-0.005B ture properties with good ...hardness, strength, and wear resistance even at ...
Hastelloy C-22 Alloy 暂无评价 23页 免费... while lowering ductility and impact properties. ...Hardness Rb 84 24c 95 Table 10 - Effect of ...
(8条) 1.Akhter J I;Shaikh M A Effect of Aging on the Hardness and Impact Properties of Hastelloy C-276[外 文期刊] 2001 2.吴嘉伟;董建新;曾燕萍...