46N.Degirmenbasietal./ColloidsandSurfacesB:Biointerfaces48(2006)42–49
Table1
AveragecrystallitesizeandfractioncrystallinityofHAp,andHAp/collagenandHAp/PVA/collagencompositesSpecimen(wt%)Plane
LinewidthFWHM( )Fractioncrystallinity,XcAveragecrystallitesize,D(nm)HAp/PVA/collagen(002)
0.458(002),(004),(130),(222)0.538HAp/collagen
(002)
0.383(002),(004),(130),(222)0.496HAp(synthesizedalone)
(002)
0.326(002),(004),(130),(222)
0.423
whentheHApissynthesizedalone,itsultimateparticlesizeisaround29.5nm.UpontheinsitusynthesisoftheHApincollagenorPVA/collagentheparticlesizedecreasestoabout24and19nm,respectively.Thedecreasingofthecrystallinityisaccompaniedbyadecreaseinthecrystallitesize(from29.5nmat40%crystallinityto19.2nmat14%crystallinity(onthebasisofthe(002)plane).ThereductionintheultimateparticlesizeofHApuponinsitusynthesisandprecipitationisconsistentwiththeresultsofRusuetal.[17],whoalsoobservedthereductionoftheparticlesizeofHApuponsynthesisinthechitosanmatrix.Forcomparison,themeanvaluesdeterminedfromtheuseoffourplanessimultaneously,i.e.(002),(004),(130)and(222)planesarealsoincludedinTable1.Similarbehaviorisobservedregardlessofwhetherthedatafromonlythe(002)planeortheequallyweigheddatafromthe(002),(004),(130)and(222)planesareutilized.
Fig.3showstheSEMmicrographsofcollagen(Fig.3(1))andHAp/collagenbiocomposite(Fig.3(2)),thepreparationofwhichinvolvedtheinsitusynthesisofHApincollagen.TheporosityofthecollagenarisesasaresultofthedryingprocesspriortotheSEManalysis.Upondryingthecollagenbecomesporous(Fig.3(1)).TheinsitusynthesisofhydroxyapatiteincollagenagaingivesrisetoaporousstructureuponthedryingoftheHAp/collagensample(Fig.3(2)).SuchHApbasedporousstructurescanoffercertainadvantagesintheareaofscaffoldsforuseintissueengineering[8]:
(a)Osteoconductivityimpartedbythepresenceofn-HApwill
generateadvantagesintheseedingofcellsandimprovetheirsurvivalandgrowthratesonscaffolds.
(b)Themechanicalpropertiesareimprovedupontheincorpo-rationoftheHApparticles.TheeffectofthecompositionofthePVAgel,usedasthebinder,ontheaveragecrystallitesizeofHApwasexamined.TheX-raydiffractionpatternsofaseriesofsamplesinclud-ingHAp(1),PVA/HApatthe15:85wt%(2),PVA/HApatthe30:70wt%(3),PVA/HApatthe50:50wt%(4),PVA/HApatthe80:20wt%(5)andPVA(6)werecollected.TheirXRDpatternsareshowninFig.4.TheaveragecrystallitesizeandfractioncrystallinityvaluesofHApweredetermined,andtheresultsaresummarizedinTable2.TheseresultssuggestthatthegreateristheconcentrationofPVAinthebiocompositesamplethesmalleristheaveragecrystallitesizeofHApandthesmalleristhecrys-tallinityofHAp.Thisresultisagainfullyconsistentwiththe
0.1419.20.1419.10.2523.80.1921.20.4029.50.35
27.6
ndingsofRusuetal.[17],whoobservedthereductionoftheparticlesizeofHApwithincreasingchitosanconcentrationintheirHAp/chitosanbiocomposites.
ItisknownthatPVAisasemi-crystallinepolymerinwhichrelativelystronginteractionsarepresentbetweenthepolymerchains,duetopresenceofthehydrogenbondsbetweenthehydroxylgroups.ThediffractionpatternofPVAisshowninFig.4(6).Thediffractionpatternrevealsanimportantdiffrac-tionpeakataround2θ=20 ,whichischaracteristicoftheorthorhombiclattice[19].AfterformingthePVA/HApbiocom-posite,thecrystallinityofthePVAphasedecreasesasshowninFig.4,indicatingthatthecrystalstructureofPVAwasindeedalteredduetothepresenceoftheHApcrystals.ThecrystallinityofthePVAissuppressedupontheinclusionoftheHApasshowninFig.4(2)–(4),presumablyonthebasisofthereductionin

the
Fig.3.(1)SEMmicrographofcollagenand(2)SEMmicrographofHAp/collagen.
Biocomposites of nanohydroxyapatite with collagen and poly(vinyl alcohol). Colloids and Surfaces B: Biointerfaces 48 (2006) 42–49 [2] R.Murugan. ...