Biocomposites of nanohydroxyapatite with collagen and poly(vinyl alcohol)

N.Degirmenbasietal./ColloidsandSurfacesB:Biointerfaces48(2006)42–4943

initschoiceasthebinder[10].However,PVAisnotgenerallybiodegradableandforvariousapplicationsPVAcanbesub-stitutedwithbiodegradablepolymerslikepoly(l-lacticacid),PLLA,andpoly(lactic-co-glycolicacid),PLGA.Cellsculturedincollagencangeneratetensionuponorientationduringgrowthtodeformthecollagenmatrixwiththeextentofthedeformationdependingontheviscoelasticpropertiesofthecollagen[11],butnoattemptwasmadeheretomodifythecollagentoimproveitsadhesionandmechanicalproperties[12]ortoguidethenucle-ationandgrowthofhydroxyapatitecrystals[13].UponsynthesisHApwasincorporatedintoPVA,followedbytheinsitusynthe-sisofHApwithinunmodi edcollagenandcollagen/PVAusingco-solutionandco-precipitationmethodstogeneratebiocom-positesofHAp/PVA,HAp/collagenandHAp/collagen/PVA.2.Materialsandexperimentalmethods2.1.Materials

CollagenoftypeIfromcalfskinwasobtainedfromSigma–AldrichChemicalCo.,USA.PVAwaspurchasedfromSigma–Aldrich,withaspeci edmolecularweightaverageof146,000–186,000,andwasspeci edtobe>99%hydrolyzed.ForthesynthesisofhydroxyapatiteCa(NO3)2·4H2OandNa3PO4wereobtainedfromSigma–Aldrich,USA,andtheNaOHandKBrwereprocuredfromMerck,Germany.ForcomparisonpurposescommerciallyavailableHApwiththeSigma–Aldrichdesignation289396andCAS#1306-06-5wasused.Allchemi-calswereusedwithoutanyfurtherpuri cation.

2.2.SynthesisofnanohydroxyapatiteandmixingwithPVAForbenchmarkingpurposes, rsthydroxyapatitewassynthe-sizedwithoutthepresenceofabinderusingamodi edversionoftheprocedureofNayarandSinha[14].Thesynthesisprocedureinvolvedthedrop-by-dropintroductionoftheCa(NO3)2·4H2Osolution(80ml,0.1M)intoaNa3PO4solution(48ml,0.1M).Thesolutionwasmaintainedthoroughlystirredatambienttem-perature.SodiumhydroxidesolutionwasaddedtomaintainthepHat10duringthecourseoftheexperiment.ThequantitiesofthereactantswereselectedtoprovideaCa/Pmolarratio,R,of1.67,suchas:

R=nCaP=1.67

wherenCaisthenumberofmolesofcalciumandnPisthenumberofmolesofPO4 3.ItisknownthatcompoundswithaCa/Pratiooflessthan1:1arenotsuitableforbiologicalimplantationapplications[15].Thesuspension,obtainedfromthereactionoftheCa(NO3)2·4H2OandNa3PO4,was lteredonB¨uchner,andthenwashedwithdeionizedwater.Theobtainedprecipitatewasdriedovernightat80 C.

Thesynthesis,carriedoutusingthisprocedure,generatesNaNO3asaby-productofthereaction,whichwasremovedupondissolutionwithdeionizedwater.FormixingofthesynthesizedhydroxyapatitewithPVA,thePVAwasseparatelyprepareduponmixingofPVAwithdeionizedwaterat90 Catvarious

water/PVAweight ratios.TheresultingviscousPVAsolutionwaskeptat90Cforabout30min.HApparticleswerethenincorporatedintothePVAsolutionundercontinuousagitationduringanother30min.TheresultingHAp-incorporatedgelwassubjectedtoonetofourcyclesofthermaltreatmentduringwhichthetemperatureofHAp-incorporatedgelwasreducedto 20 Candthenincreasedbackto20 Cateachcycle.Thewatercontentofthegelsampleswascontinuouslymonitoredusingthermogravimetricmethods.Thedynamicpropertiesofthehydrogelsampleswerecharacterizedduringthethermaltreatmentaswellasinbetweendifferentthermalcycles.

2.3.Synthesisofhydroxyapatite/collagenbiocompositeinsitu(HAp/Col)

First,30mlmixtureofcollagen/waterwaspreparedatacolla-genconcentrationof0.6mg/mlunderroomtemperaturecondi-tionsandcontinuousstirringfor2h.Second,thiscollagen/watermixturewasaddedinto80mlof0.1MCa(NO3)2·4H2O.Third,Na3PO4(48ml,0.1M)solutionwasthenaddedslowlyandthepHwasadjustedto10usingsodiumhydroxide.Thecol-lagen/HApmixtureatthisstageappearedasahydrogel.Thishydrogelconstitutedthecollagen/HApbiocompositeandwas lteredonB¨uchner,washedwithwater,collectedanddriedatroomtemperatureandcharacterized.

2.4.Synthesisofhydroxyapatite/collagen/PVAcompositeinsitu(HAp/collagen/PVA)

Firstamixtureofcollagen/water/PVAwasprepared.ThisprocedureinvolvedthemixingofTypeIcollagen(fromcalfskin)withwatertoreachaconcentrationof0.3mg/mlatroomtemperatureuponstirringforabout1h.Thecollagen/watermix-ture(0.3mg/ml)wasthenaddedintothePVA/watermixture(atequalvolumes).Theresulting30mlmixturewasthenstirredatroomtemperatureforatotaldurationof30min.Second,40mlof0.1MCa(NO3)2wasaddedtothePVA–collagenmixture(pHadjustedto10),mixed,heldat70 Cfor24h.Third,24ml0.1MNa3PO4(pHreadjustedto10)wasaddedtothemixture.TheHApthussynthesizedinsituinthecollagen/PVAbinderwasseparated, ltered,washed,driedandcharacterized.Itshouldbenotedthatthisprocedure(unlikeuponsynthesisincolla-genwhichconservesthecollagenstructurediscussedearlier)denaturesthecollagenintogelatin,however,forthesakeofcon-veniencewewillcontinuetorefertothebiocompositeobtainedasHAp/collagen/PVAforbothcases.

2.5.Linearviscoelasticbehaviorusingsmall-amplitudeoscillatoryshear

Thelinearviscoelasticmaterialfunctionswerecharacterizedusing25mmparallelplatesundersmall-amplitudeoscillatoryshearinconjunctionwithanAR2000ARESrheometerfromTAInstruments.

Therelationshipbetweentheshearstress,τyx(t),andthestrain,γyx,imposedonthematerialduringsmall-amplitude

上一页第2页

你可能喜欢

热门文档

相关文档

  • 纳米羟基磷灰石

    Biocomposites of nanohydroxyapatite with collagen and poly(vinyl alcohol). Colloids and Surfaces B: Biointerfaces 48 (2006) 42–49 [2] R.Murugan. ...

  • 纳米羟基磷灰石

    Biocomposites of nanohydroxyapatite with collagen and poly(vinyl alcohol). Colloids and Surfaces B: Biointerfaces 48 (2006) 42–49 [2] R.Murugan. ...