Investigation of tribological properties of Al2O 3-polyimide nanocomposites

876H.Caietal./PolymerTesting22(2003)875–882

effectofinorganicnanometer lleronthetribologicalpropertiesofpolymermatrixcompositesandthemech-anismsofvarious llershavebeenroughlyrecognized[12,19].

Accordingly,thetribologicalpropertiesofPI-basednanocompositesincorporatingdifferentproportionsofnanometerAl2O3particlesaredealtwithinthepresentwork,byslidingthePInanocompositeblocksagainstaplaincarbonsteelring.

2.Experimental

2.1.Materialsandspecimens

4,4’-oxydianiline(ODA)anddiphenylether-3,3’,4,4’-tetracarboxylicdianhydride(OPDA)werepurchasedfromcommercialsourcesanddriedbeforeuse.Nano-meterAl2O3wasalsocommerciallyobtainedfromanan-ometermaterialcorporationinShandongProvinceofChina.Theothercompoundsincludingtriethylamine,pyridine,N-methyl-2-pyrrolidone(NMP)etc.,werecom-mercialanalyticalgradereagentsandusedwithoutfurtherpuri cation,exceptthatNMPwasdriedovermolecularsievesbeforeuse.

Poly(amicacid)solutionwasobtainedbyaddinganequimolaramountofOPDAtoanODA/NMPsolution.ThehomogeneoussuspensionsofAl2O3/NMPwithdif-ferentAl2O3proportionswereaddedintoPAAsolutionundervigorousagitation.ThehomogeneoussuspensionofAl2O3/PAA/NMPwasprecipitatedbyintroductionoftriethylamineandpyridine.Afterdryingtoallowthermalimidization,PI/Al2O3powderswerecompressedandheatedto340°Cinamoldatarateof8°C/min.Thepressurewasheldat10MPabelow315°Candraisedto25MPafortherestoftheheatingcycle,toensuregoodcompactingoftheresultantcompositespecimens.Thecompressedcompositewasheldat340°Cfor10minandthencooledto100°Cinthemold.Afterreleas-ingfromthemold,theresultantblockspecimenswereusedforfrictionandweartests.2.2.Characterization

Themicrohardnessofthespecimenswasdeterminedbyconducting vereplicatemeasurementsonanMH-5microhardnessmeter,ataloadof2Nandaloadingtimeof5s.Theaverageofthe vereplicatemeasurementsofthehardnessvaluesiscitedasthehardnessofthespecimen.

ThebendingstrengthofthePI/Al2O3nanocompositeswasmeasuredusinganAG-10TAuniversalmaterialtes-ter(ShimadzuCorporationofJapan)inaccordancewithnationalstandard

Investigation of tribological properties of Al2O 3-polyimide nanocomposites

GB9341-88.

Fig.1.Contactschematicdiagramforthefrictionalcouple.

2.3.Frictionandweartest

ThefrictionandweartestswereconductedonanM-2000modelfrictionandweartester.Thecontactsche-maticdiagramofthefrictionalcoupleisshowninFig.1.Aplaincarbonsteelring(HRC48–50)withdiameterof40mmwasusedasthecounterpart.Slidingwasper-formedunderambientconditionsoveraperiodof1.5hatslidingvelocitiesof0.431m/sand0.862m/s,normalloadof50N,100N,200N,and290N.Theambienttemperaturewasroughly25°Candtherelativehumidityabout50%±10%.Beforeeachtest,thesurfacesoftheblockspecimensandcounterpartringwereabradedwithNo.900water-abrasivepaper.Then,thesteelringwascleanedwithacetone-dippedcottonandthePIoritsnan-ocompositeblockswerecleanedwithacetone,followedbydrying.Thefrictionforcewasmeasuredusingatorqueshaftequippedwithstraingauges,andthefrictioncoef cientcalculatedbytakingintoaccountthenormalloadappliedandthefrictionforcemeasured.Attheendofeachtest,thewidthofthewearscarontheblockspecimenswasmeasuredwithadigital-readingmicro-scope,thenthewearvolumelossVoftheblockspeci-mencalculatedfromtherelationship:

V B·

pR2180·arcsin b

2R b2

R2

b2

4

,

whereVreferstothevolumeloss(mm3),Btothewidthoftheblockspecimen(mm),Rtotheradiusofthesteelring(mm),andbtothewidthofthewearscar(mm).Threereplicatefrictionandweartestswerecarriedout

上一页第2页