Fig.1.TypicalP-hcurvesofBMGsbyrate-jumpnanoindentationtestingat

avarietyofloadingrates.AninstrumentedindentationapparatusequippedwithaBerkovichindenterwasusedforthemechanicaltests.AkintotheexampleBMGshownhere,allBMGsinvestigatedinthisstudyexhibitweakyetdiscernableratedependenceoftheirmechanicalresponse.

ResultsandDiscussion

Inthisstudy,wedevelopedarate-jumpnanoindentationmethodtocharacterizethestrainratesensitivityofhardness.Inajump-rationanoindentationexperiment,multistepload–unloadcycleswithvariousloadingratesareimplementedinthecourseofonenanoindentationexperimentinanefforttominimizepossibletest-to-testvariationscausedbyseparatehardnessmeasurementsatdifferentloadingrates(seeMethods).Fig.1Ashowstypicalmulti-stepforce-depth(P-h)curvesforoneofthesixBMGsinvestigatedherein.Thehardnessiscalculatedasafunctionofindentationdepth(Fig.1B)(24).ItcanbeclearlyseeninFig.1Bthatthehardnessincreasesuponloadingatahigherloadingrate.How-ever,theincrementinhardnesswithincreasingloadingrateismild,displayingconformitywiththeobservationintheliteraturethattheratedependenceof owstressisminororevennegligibleinplastic owkineticsinmetallicglasses(9,12).

AsshowninEq.6,onecriticalparameterindeterminingtheSTZvolumesofBMGsbymeansofnanoindentationisthestrainratesensitivity,m.Innanoindentationexperiments,thehardness

H=

PYh2,[7]

p

wherehp=ht CP

isthetotalindentationistheplasticdepthatappliedforceP;ht

depthatP;CandYareindentershape-dependentconstants;anddP/dhisthecontactstiffnessatP.At

Experimental characterization of shear transformation zones for plastic flow of metallic glasses

a

14770doc.guandang.net

Fig.2.Determinationofratesensitivityofhardness/strengthofBMGs.Loadingratesrangingfrom13.2mN/sto264.0mN/swereadopted.FollowingEq.6,equivalentstrainratesaredeterminedforcalculationofratesensitivity.Extremecarehasbeenexercisedforaccuratemeasurementsofthisimportantparameterinidenti cationofSTZvolumesofplastic owofBMGs.

peakloadPofaload–unloadcyclewherethedeterminedhardnessdoesnotaltermarkedlywithindentationdepthordeformation

time,assumingtheequivalentstrainrateε˙=1dh

pp(25–27),wehave

P˙=dPdt=d(YHh2p)dt=2YHhdhppdt=2YHh2pε˙=2Pε˙.[8]

Therefore,theequivalentstrainrate

ε˙=P

˙/2P[9]

Thecorrespondingstrainratesensitivityofhardnessishenceextractedbyliningupthehardnessvs.equivalentstrainrateinalog–logscaleandmeasuringtheslopeoftheline(Fig.2).TheSTZsizesofthesixspecimenmetallicglassesareconse-quentlycalculatedbyusingEq.6,theresultsofwhicharelistedinTable1.Inadditiontotherate-jumpnanoindentationexper-imentsasdepictedabove,aparallelexperimentalprocedure,separatehardnessmeasurementsatavarietyofloadingrates,hasalsobeenindependentlyappliedtocharacterizethestrainratesensitivityofhardnessofBMGs[seesupportinginformation(SI)TextandFigs.S1andS2].Wecomparedtheresultsobtainedbythetwomethodsandaremarkableagreementisfound.Forinstance,forPt57.5Cu14.7Ni5.3P22.5,thehardnessdeterminedbytherate-jumpandseparate-indentationmethodsis5.31GPaand5.32GPaatequivalentstrainrateof0.05s 1,respectively,whereasthecorrespondingstrainratesensitivitiesare0.0096and0.0089,respectively.

AsshowninTable1,theratesensitivitiesofhardness/strengthofBMGsaregenerally<0.03,whichindicatesanearlyidealplas-ticdeformationintheinhomogeneous owandisconsistentwiththeinsigni cantratedependenceofstrengthofBMGsreportedintheliterature(9,12,28).AlthoughthestrainratesensitivityofthePd40Ni40P20sampleisaslowas0.0067,thecapabilityofnanoindentationtoaccuratelymeasuresuchlowratesensitivitieshasbeenvalidatedinourpreviouswork(24)anda niteelementanalysis(seeSITextandFig.S3).Inthisstudy,largeindentationforcesareselectedforthepurposeofminimizingpossibleeffectstothemeasuredBMGhardnessfromfactorssuchasindentationsize(e.g.,Nix–Gaorelationinindentationsize),indenterimper-fections,surfaceroughness,andpop-ineventsatsmallloadsandlowloadingrates(30–34).Moreover,theaveragehardnessisusedinthecalculationsofthevolumesofSTZsinthemodelBMGsystems,providedthatthein uenceofthehardnessvariation