Inducement-of-bainite-and-carbide-transformation-from-retained-austenite-based-on-a-high-strain-rate

H.-C.Hsuetal./ScriptaMaterialia62(2010)372–375

373

Table1.Chemicalcompositionof300Msteel.ElementCMnSiCrContent(wt.%)

0.41

0.81

1.61

0.83

dimensions,anddirectlyoilquenchedat40°C.Thequenchedspecimenswerethendoubletemperedat280°Cfor2h.Cylindricalcompressionspecimens10mminheightand10mmindiameterwerepreparedfromthebars.Allspecimensurfacesonbothendswerecarefully nishedtoensureclosecontactthepressurebarsduringimpactdeformation[9].Dynamiccompres-siontestswereperformedatstrainratesof1Â103s–1and4Â103s–1atroomtemperaturethroughmeansofaSplitHopkinsonPressureBar(SHPB).Moreover,thinfoilswerepreparedfromtheimpactedspecimensfortransmissionelectronmicroscope(TEM)examination.Diskswithadiameterof3mmwerepunchedfromthoseof0.05mmthinslices.Thediskswereelectropolishedtoathinfoil,atatemperaturebelow15°C,inasolutioncomposedof100gchromictrioxide,540cm3glacialace-ticacid,and28cm3distilledwater.Voltagesof35Vfortheinitialpolishingand55Vforthesecondpolishingwereusedatacurrentdensityof0.1–0.2Acm–2.

Opticalmicrostructuresofthe300Msteelwereevalu-atedafterdynamicimpacttestsattwostrainrates,i.e.1Â103s–1and4Â103s–1.The neimpactedmicrostruc-turesofthesamplesdeformedatthetwostrainratescon-sistofpacketbainite.Atahigherstrainrateof4Â103s–1,grainsinsomepacketsexhibitsignsofcoarsening.Thede-greeofdeformationfromtheheightreductionisaround1%engineeringstrain3at1Â103s–1and14%engineeringstrainat4Â10s–1.Themicro-hardnessdistributionsacrossthediameteroftheas-receivedandimpactedmate-rialsexhibituniformityforbothstrainrates.Theaveragehardnessvalueofthe300Msteelimpactedat1Â103s–1isapproximately285Hv,i.e.nearlythesamevalueasthatoftheas-received300Msteelin286Hv.Thesigni cantincreaseinhardnesswith331Hvatahighstrainrateof4Â103s–1isassociatedwithgreatertruestress–truestraincurves(Fig.1).Ahigherstrainhardeninge ectresultinginagreater owstresswasexhibitedatastrainrateof4Â103s–1(Fig.1).Asimilartrendhasbeenob-servedinimpactedduplexstainlesssteelandsuperausten-iticstainlesssteel[7].

Figure1.Dependenceofimpactstrainrateontrue owstressof300M

Inducement-of-bainite-and-carbide-transformation-from-retained-austenite-based-on-a-high-strain-rate

steel.NiMoCuSPV

1.86

0.38

0.04

0.001

0.005

Inducement-of-bainite-and-carbide-transformation-from-retained-austenite-based-on-a-high-strain-rate

0.065

Duringhighstrainratedeformation,thetemperatureriseinthespecimenisowingtotheinsu cienttimetoconductawaytheadiabaticheatgeneratedbytheplasticwork.Owingtothedi cultyofmeasuringthistemper-atureriseexplicitlyduringahighvelocityimpact,themagnitudeoftemperatureriseisestimatedbyaninte-gralequationDT¼ [10]instead:

1

Ze

qCrde

p0whereDTdenotesthetemperaturerise,qrepresentsthe

density(7.83gcm–3),C°C–1),risthepreferstotheheatcapacity(0.114calg–1stress,anddeistheintervalofstrain.ThecalculatedtemperaturesfromFigure1are46°Catastrainrateof1Â103s–1and87°Catastrainrateof4Â103s–1.Theaboveresultsprovidefurtherin-sightintotheapparentsofteningandassociatedphasetransformation.

TheTEMmicrostructureofas-received300Msteelconsistsofbainiticferriteplateletswithcarbon-enrichedretainedausteniteinbetween(Fig.2).Nocarbidesarepresentbecausethehighsiliconcontentin300Msteel,1.6wt.%,inhibitstheformationofthecarbideFe3C,sub-sequentlycausingthecarbon-enrichedretainedaustensiteandbainite[8].Siliconhasanextremelylowsolubilityincementite.Owingtotheabilityoftheparaequilibriumtransformationtoinheritthesilicon,thedrivingforceforprecipitationismarkedlyreduced,subsequentlyretardingprecipitation[11].Inadditiontoa ectingthemechanicalproperties,thevariationofphysicalbehaviorcausedbydynamicimpactalsoa ectsthemicroscopicstructure.Whenthesteelwasimpactedatalowerstrainrateof1Â103s–1,thecoarsebainiteplatesintheas-re-ceivedmaterial(Fig.2)wascompressedintothinbainiteplatesasdepictedinFigure3a.Theretainedaustenitewastransformedintostress-inducedupperbainiteunderabout1%strain(Fig.3a).Althoughtheretainedaustenitecantransformintobainitewithannealingforanextendedperiodattemperaturesexceeding150°C[12],bainitedis-placivetransformationoccurredatalowertemperature

Figure2.Quenchedanddoubletempered300MsteelTEMmicro-structureofbainitewithretainedaustenitebetweenplates.