NaYF4:Yb3+,Er3+(Tm3+)/PMMABulkNanocompositesformationofthenanocomposites.Theas-preparednanocom-positeswithoutintroducingstabilizerhaveanadvantageinthatthemechanicalpropertiesofthenanocompositesarenotin uencedbyinterfacialinteractionbetweenthePMMAandthestabilizer.Themorphology,structure,thermalstability,mechanical,luminescent,andenergytransferpropertiesofthesenanocompositeswereinvestigatedindetail.Theobtainedcompositematerialsshowstronggreenorbluephotolumines-cenceunder980nmexcitationandaretransparentinthevisibleregion.
2.ExperimentalSection
Materials.Y2O3(99.999%),Yb2O3(99.999%),Er2O3(99.999%),andTm2O3(99.999%)werepurchasedfromScienceandTechnologyParentCompanyofChangchunInstituteofAppliedChemistry.Methylmethacrylate(MMA,99%),oleicacid,andtri uoroaceticacid(99%)werepurchasedfromSinopharmChemicalReagentCo.,Ltd.1-OctadecenewasobtainedfromAldrich.Sodiumtri uoroacetate,butanediolmonoacrylate(BDMA),trimethylolpropanetriacrylate(TMP-TA),andphotoinitiator2,4,6-trimethylbenzoyldiphenylphos-phineoxide(TPO)wereobtainedfromTCI(Tokyo,Japan)andusedasreceived.Rareearthtri uoroacetateswerepreparedbydissolvingthecorrespondingrareearthoxidesintoamixedsolutionofwaterandtri uoroaceticacid(50:50byvolume)andthenevaporatingthesolvent.
Preparationof -NaYF4:17%Yb3+,3%Er3+and -NaYF4:25%Yb3+,0.3%Tm3+Nanoparticles.AllofthedopingratiosofLn3+aremolarinourexperiments.The -NaYF4:17%Yb3+,3%Er3+and -NaYF4:25%Yb3+,0.3%Tm3+nanoparticlesemployedinthisstudyweresynthesizedaccordingtotheliteraturemethod.13Forthesynthesisof -NaYF4:17%Yb3+,3%Er3+,2.06mmolCF3COONa,0.75mmolY(CF3COO)3,0.16mmolYb(CF3COO)3,and0.03mmolEr(CF3COO)3weremixedwith60mmololeicacidand60mmol1-octadeceneina250mLthree-necked ask.Thesolutionwasheatedto100°Ctoremovewaterandoxygen,withvigorousmagneticstirringundervacuumfor30min,andthenheatedto325°Candmaintainedfor1.5hunderArgonprotection.Afterthesolutionwascoolednaturally,nanocrystalswerecentrifugallyseparatedfromthesolutionwithethanolandwashedwithethanolthreetimes.Similarly, -NaYF4:25%Yb3+,0.3%Tm3+nanocrystalsweresynthesizedusingY(CF3COO)3,Yb(CF3COO)3andTm(CF3COO)3withamolarratioof0.747:0.25:0.003.
Preparationof -NaYF4:17%Yb3+,3%Er3+/PMMAand -NaYF4:25%Yb3+,0.3%Tm3+/PMMANanocomposites.MMA(2.3g)wasmixedwith0.8gofBDMAand0.8gofTMPTA.Tothissolution,0.1wt%(0.0039g)ofNaYF4:Yb3+,Er3+(Tm3+)nanoparticleswereadded.Thesolutionwassonicatedfor10mintodispersethenanoparticles.AfterphotoinitiatorTPOwasaddedtothesolutions,theparticledispersionsinmonomersweretransferredintoaglassmoldformedbyseparatingtwoglassplateswiththickglassseals,andtheglasstemplateswereheatedto50°Cbeforeuse.PolymerizationwascarriedoutinaUVinertcubeusingUVradiation(200Wcm-1,LAMP,PHILIPS)for5min.Differentdopingconcentrations(0.5and1wt%)ofNaYF4:Yb3+,Er3+(Tm3+)nanoparticlesinnanocompositeswereselectedtoinvestigatetheeffectofthefactoronthetransparenceandopticalproperties.
Characterization.X-raydiffractions(XRD)ofthepowdersampleswereexaminedonaD8Focusdiffractometer(Bruker)usingCuKRradiation(λ)0.15405nm).Scanningelectronmicroscopy(SEM)micrographsandenergy-dispersiveX-ray
J.Phys.Chem.C,Vol.114,No.1,2010611
Figure1.XRDpatternsofNaYF+4:17%Yb3+,3%Er3+andNaYF4:25%Yb3,0.3%Tm3+nanoparticles.Thelinespectrumcorrespondstothestandarddataof -NaYF4(JCPDSNo.16-0334).
spectroscopy(EDS)weremeasuredona eldemissionscanningelectronmicroscope(FE-SEM,XL30,Philips).Thenanocom-positesampleswerecryogenicallybrokenafterimmersioninliquidnitrogen,andthefracturedsurfaceswerecoatedwithPtandobservedbyanSEM.Transmissionelectronmicroscopy(TEM)wereperformedonaJEOL-2000TEMoperatingat200kV.SamplesforTEMwerepreparedbydepositingadropofacolloidalethanolsolutionofthepowdersampleontoacarboncoatedcoppergrid.Theexcessliquidwaswickedawaywith lterpaper,andthegridsweredriedinair.Thethermogravi-metricanalysis(TGA)datawererecordedwithaThermalAnalysisInstrument(PyrisDiamond,PerkinElmer)withaheatingrateof10°C/mininair.FlexuraltestswerecarriedoutatroomtemperaturebyusinganInstronmechanicaltestinginstrument(INSTRON-1121).Theultraviolet-visible(UV-vis)transmissionspectraweremeasuredonaTU-1901spectropho-tometer,andtheas-preparedbulknanocomposites(35×15×2mm)weremeasuredwithoutanyprocessing.Theupconver-sionemissionspectrawereobtainedusinga980nmlaserfromanopticalparametricoscillator(OPO,ContinuumSurelite,USA)astheexcitationsourceanddetectedbyanR955(HAMAMAT-SU)from400to850nm(thepowerdensityusedwasabout6Wcm-2).ThephotoluminescencelifetimesofthesamplesweremeasuredwithaLecroyWaveRunner6100DigitalOscilloscope(1GHz)usingatunablelaser(pulsewidth)4ns,gate)50nm)astheexcitationsource(ContimuumSunliteOPO).Allthemeasurementswereperformedatroomtemperature.3.ResultsandDiscussion
3.1. -NaYF4:17%Yb3+,3%Er3+and -NaYF4:25%Yb3+,0.3%Tm3+Nanoparticles.ThesynthesisofNaYF4:Yb3+,Er3+(Tm3+)nanoparticleswasadoptedfromMaietal.13withalittlechange.TheNaYF4reportedintheliteratureishexagonalnanoplateswithsizeof200nm.Thebiggerparticlesaredif culttodispersewellinthesolvent.Weloweredthereactiontemperature(325°Cforourexperimentand330°Cfortheliterature)andextendedthereactiontime(1.5hforourexperimentand30minfortheliterature).Asaresult,westillgotpure-phase -NaYF4(Figure1)whoseparticlesizedecreasedtoaround40nm.ThephasestructuresofthenanoparticleswereinvestigatedbyXRD.Figure1showsXRDpatternsofNaYF4:17%Yb3+,3%Er3+andNaYF4:25%Yb3+,0.3%Tm3+nanoparticlesandthestandarddatafor -NaYF4aswell.TheresultsoftheXRDindicatethattheas-formedNaYF4:17%Yb3+,3%Er3+andNaYF4:25%Yb3+,0.3%Tm3+samplesare

well
Preparation and Upconversion Luminescence of Y3Al5O12 : Yb 3+ , Er 3+ Trapsparent Ceramics_专业资料。维普资讯 http://www.cqvip.com M n .U 量Aalbl...
Preparation and upconversion luminescence of YVO4:Er 3+,Yb 3+_专业资料。Ienina oralfMirl,ntratolun JoneasMetlga trasaly ndMaeil ur...
and Characterization of Upconversion Fluorescent Yb3...[3–9], which are based on luminescent ...(C) Preparation of the Fluoride Containing ...
upconversion emission of ZrO2-Er3+ nanocrystals_...Sample preparation The samples were prepared by ...2.3. Photoluminescence characterization The ...
Er3+ Ho3+ upconversion_物理_自然科学_专业资料。Energy transfer upconversion...Edelstein, “Preparation of cubic chloro complex compounds of trivalent metals...
Journal of Alloys and Compounds 397 (2005) 1–4 Synthesis and NIR-to-violet, blue, green, red upconversion ?uorescence of Er3+:LaOBr Dianyuan Wang ...
912 Chemistry Letters Vol.36, No.7 (2007) Bright Green Upconversion Fluorescence of Yb3? , Er3? -codoped Fluoride Colloidal Nanocrystal and ...
NaYF4_Yb3+_Er3+上转换荧光标记纳米晶的制备与性能表征_化学_自然科学_专业...Preparation and Characterization of Upconversion Luminescent NaYF 4 :Yb3+, Er...
Upconversion Luminescence of Monodisperse CaF2Yb3+Er3+ Nanocrystals_能源/化工...In addition, these luminescent properties show that these water-soluble CaF2...
Spectroscopy, upconversion dynamics, and applications of Er3+-doped low-...luminescent solids is also discussed, paying especial attention to new ...
热门文档