Recycled Tyre Rubber Modified Bitumens for road asphalt mixtures_ A literature review

872

Table7

Caltransspeci cationforrubberisedbitumen[36].Testparameter

Apparentviscosity,Haake,190°C:cp

Conepenetrationat25°C(ASTMD217):dmmSofteningpoint(ASTMD36):°C

Resilienceat25°C(ASTMD3407):%

D.LoPresti/ConstructionandBuildingMaterials49(2013)863–881

Table9

Rubbercrumbsrequirementsforbitumen–rubber,adaptedfrom[38].

Speci cationlimits1500–400025–7052–74

Minimum18

Property

Sieveanalysis(%mass)Passingscreen(mm)1.1800.6000.075

Poly-isoprenecontent(%m/mtotalhydrocarbon)Fibrelength(mm)Bulkdensity(g/cm3)

Requirement

TestmethodMB-14

10040–700–525min6max1.10–1.25

ThermogravimetricAnalysisMB-16

viscosityoftheAsphalt-Rubberinteractionovertimeforqualitycontrolandassurance.BeforeanyAsphalt-Rubberbindercanbeused,compliancewiththeminimumviscosityrequirementmustbeveri edusinganapprovedrotationalviscometer(e.g.Brook- eld).Aslongastheviscosityisincomplianceandtheinteractionhasproceededforatleast45min,theAsphalt-Rubbermaybeused[36].

Caltrans(2006)recognisesthatbeforestartingtheplantpro-duction,anappropriateAsphalt-Rubberbinderdesignmustbedeveloped(Table7).Italsospeci esthatatleast2weekspriortostartofconstructiontheContractormustsupplytotheEngineer,forapproval,anAsphalt-Rubberbinderformulation(designor‘‘recipe’’)thatincludesresultsofspeci edphysicalpropertytests,alongwithsamplesofallofthecomponentmaterials.SamplesofthepreparedAsphalt-RubberbindermustalsobesubmittedtotheEngineeratleast2weeksbeforeitisscheduledforuseontheproject.

3.1.4.Asphalt-Rubberstorage

CaltransrequiresheatingtobediscontinuedifAsphalt-Rubbermaterialisnotusedwithin4hafterthe45-minreactionperiod.Therateofcoolinginaninsulatedtankvaries,butreheatingisre-quiredifthetemperaturedropsbelow190°C.Areheatcycleisde- nedasanytimeanAsphalt-Rubberbindercoolsbelowandisreheatedto190–218°C.Caltransallowstworeheatcycles,buttheAsphalt-Rubberbindermustcontinuetomeetallrequire-ments,includingtheminimumviscosity.

Sometimesthebindermustbeheldovernight.ThebitumenandrubberwillcontinuetointeractatleastaslongastheAsphalt-Rub-berremainsliquid.Therubberbreaksdown(isdigested)overtime,whichreducesviscosity.Upto10%moreCRMbybindermasscanbeaddedtorestoretheviscositytospeci edlevels.TheresultingAsphalt-Rubberblendmustbeinteractedat190–218°Cfor45minandmustmeettheminimumviscosityrequirementbeforeitcanbeused.

3.2.BitumenRubberbinder(RSA)

BitumenRubberbinderisaterminologyusedfortherubberisedbitumenobtainedbythewetprocessinSouthAfrica.BitumenRubberbinderscombinerubbercrumbs(Table9)withbitumen

athightemperaturestoachieveacomplextwophaseproduct,namednon-homogeneousbinder.IntheTechnicalGuidelineoftheSouthAfricanAsphaltAcadamey[38],isalsoreportedthatpropertiesofthemodi edbinderusedinhotmixasphaltwillin uencetheengineeringpropertiesoftheresultantmix,thereforethesubstitutionofaconventionalbitumenwithamodi edbindercanresultinhigherairvoidsduetoreducedworkabilityofthehigherviscositymodi edbinders.Forthisreason,itisimportantthatsplitsamplesofthemodi edbinderaresenttoallthepartic-ipatinglaboratories(e.g.:supplier,siteandcontrollaboratories)andtestedbeforecommencementofaprojecttoensurethattheresultsarewithinthereproduciblelimitsasprescribedbythetestmethods.

3.2.1.Rubberrequirements

InSouthAfrica,theCommitteeofLandTransportOf cials(COL-TO)’sspeci cationrequiresthereclaimedrubbertohavenotlessthan30%naturalrubberbymassofhydrocarboncontent[39],whilsttheSABITAManual[40]andtheTechnicalGuidelineoftheSouthAfricanAsphaltAcadamey[38]specify60–75%naturalrubberbymassofhydrocarboncontent,withallrubberparticlespassingthe1.18mmsieve.TheCRMisproducedbyamechanicalsizereductionprocess.CRMproducedbycryogenic-mechanicaltechniquesarenotpermittedinSouthAfrica.TheCRMmustbepulverised,freeoffabric,steelcordsandothercontaminants.3.2.2.Basebitumenrequirements

Thebinderusedintheproductionofthebitumen–rubbermustbeSABITAB12orB8road-gradebitumen(60/70or80/100pene-tration-gradebitumenrespectively)orablendofthesegradestoprovideaproductwithaparticularviscosityandotherprescribedproperties.

3.2.3.BitumenRubberproduction

Thebinderismanufacturedfromblendingpenetrationgradebitumen(72–82%bymass),plusextenderoil(0–4%)plusrubbercrumbs(18–24%)inapatentedhighshearmixerwithaspeedof

Table8

Speci cationforAsphalt-Rubber[37].Binderspeci cation

ASTMD6114(2009)TypeI

Apparentviscosity177.5°C(ASTMD2196):cpPenetrationat25°C(ASTMD5):dmmPenetrationat4°C(ASTMD5):dmmSofteningpoint(ASTMD36):°C

Resilienceat25°C(ASTMD5329):%Flashpoint(ASTMD93):°C

AfterTFOT(ASTMD1754),residualpenetrationat4°C(ASTMD5):%Climaticregion

Averageminimummonthlytemperature:°CAveragemaximummonthlytemperature:°C

1500–500025–75Min10Min57.2Min25Min232.2Min75HotMinÀ1Min43

TypeII1500–500025–75Min15Min54.4Min20Min232.2Min75ModerateMinÀ9Max43

TypeIII1500–500050–100Min25Min51.7Min10Min232.2Min75ColdMinÀ9Max27