文档下载 文档下载导航
设为首页 | 加入收藏
搜索 请输入内容:  
 导航当前位置: 文档下载 > 所有分类 > 工程科技 > 能源/化工 > Cycling degradation of an automotive LiFePO4 lithium-ion battery
侵权投诉

Cycling degradation of an automotive LiFePO4 lithium-ion battery

lithium secondary batteries.

JournalofPowerSources196 (2011) 1513–1520

ContentslistsavailableatScienceDirect

JournalofPower

Cycling degradation of an automotive LiFePO4 lithium-ion battery

Sources

journalhomepage:doc.guandang.net

Cycling degradation of an automotive LiFePO4 lithium-ion battery

r

CyclingdegradationofanautomotiveLiFePO4lithium-ionbattery

YanchengZhanga,Chao-YangWanga, ,XidongTangb

ElectrochemicalEngineCenter(ECEC),DepartmentofMaterialsScienceandEngineering,andDepartmentofMechanicalandNuclearEngineering,ThePennsylvaniaStateUniversity,UniversityPark,PA16802,USAb

GMR&DandPlanning,GeneralMotors,MailCode:480-106-390,30500MoundRoad,Warren,MI48090-9055,USA

a

articleinfoabstract

DegradationofahighcapacityprismaticLiFePO4cellwithdeepcyclingatelevatedtemperatureof50 Cisstudiedbyelectrochemicalimpedancespectroscopyaswellascapacityandpowerfadingcharacteri-zationatdifferenttesttemperatures(45,25,0and 10 C).Capacityfadeafter600cyclesis14.3%at45 Cand25.8%at 10 C.Thereislittlepowerfadeat45 Cafter600cycles,whereasthepowerfadeafter600cyclesis61.6%and77.2%,respectively,at0and 10 C.Thecapacityandpowerfadeevidentlybecomesmoresevereatlowertemperature.Inparticular,thepowerfadeatlowtemperatures(e.g.,0and 10 C)ratherthancapacitylossisamajorlimitationoftheLiFePO4cell.Theprimarymechanismforcapacityfadeislossofcyclablelithiuminthecellresultingfromlithium-consumingsolidelectrolyteinterphase(SEI)layergrowthandsidereactions.Theincreasedinterfacialresistance(Rw)duetothecatalyticgrowthofSEIlayeronthegraphiteanodeandincreasedelectrolyteresistancearethemainsourcesforpowerfade.

© 2010 Elsevier B.V. All rights reserved.

Articlehistory:

Received9July2010

Receivedinrevisedform20August2010Accepted23August2010

Available online 22 September 2010Keywords:LiFePO4

Lithium-ionbatteryCyclingdegradation

ElectrochemicalimpedancespectroscopyElectric-onlyrange

1.Introduction

LithiuminsertionandextractioninaLiFePO4cathodeinvolvea rst-orderphasetransitionbetweentwophases(FePO4andLiFePO4)[1],eventhoughthetwo-phasereactiontheorywaschal-lengedathightemperatures(forinstance,heatingupto200 C[2])andfornano-particles(<50nm[3]).BothFePO4andLiFePO4phaseshavelowelectronicconductivity[4,5],andslowdiffusionoflithiumionsthroughthetwo-phaseinterfacelimitsthechargeanddischargecurrentdensity[1].ThesecausepoorpowercapabilityandlowcapacityofLiFePO4batteries.Theelectronicconductiv-ityhasbeensigni cantlyincreasedfrom10 9–10 10Scm 1to10 2Scm 1since2002[5]butthemechanismfortheenhance-mentisunderdebate[6–8].Extensiveliteraturedemonstratesthatcarbon-coatinganddecreasingparticlesize(orincreasingspeci csurfacearea)areeffectiveapproachestoovercometheproblemoflowelectronicandionicconductivitiesinLiFePO4cathode[9–20].Inparticular,carbon-coatedLiFePO4(C-LiFePO4)wasclaimedtoachievehighcapacity(e.g.,90%oraboveofthe170mAhg 1theo-reticalcapacity)andexcellentcyclingperformance[10–12].TheattractivepropertiesofC-LiFePO4asacathodematerialhaveenabledahigh-powerlithium-ionbatterywithhighsafety,lowcostandlonglife,anditscommercializationcanofferwideapplica-tionsespeciallytohybridelectricvehicles(HEVs)andplug-inHEVs(PHEVs).

Correspondingauthor.Tel.:+18148634762;fax:+18148634848.E-mailaddress:cxw31@psu.edu(C.-Y.Wang).0378-7753/$–seefrontmatter© 2010 Elsevier B.V. All rights reserved.doi:10.1016/j.jpowsour.2010.08.070

Excellentlong-termcyclingstabilitywasdemonstratedforC-LiFePO4/graphiteprismaticcellswithcapacitylossofonly14%after6000charge–dischargecycles[21],wherethecellswerecycledat20 Candaround1Crate.However,high-temperaturecyclingsig-ni cantlyacceleratedcapacityfading[22].Amineetal.reportedthattherewaslittlecapacityfadeat25 C,butapproximately70%capacitylossat55 Cafter100charge–dischargecyclesatC/3rate[22].Thefastfadingathightemperatureswasfoundtoresultfromformationandgrowthofthickinterfacial lmandconcomitantlargeimpedanceriseonthegraphiteanodewhichwascatalyzedbyirondepositiononthegraphiteanodesubsequenttoirondisso-lutionfromtheLiFePO4cathode[22–24].Asperthismechanism,usingLi4Ti5O12anodeinsteadofgraphiteanodesloweddownirondepositionontheanodewithahighpotentialofca.1.5VversusLi+/Li[22],andion-sievingmetalcoating(30–50nmAuorCucoating)ongraphiteanodereducedsolidelectrolyteinter-phase(SEI)formationonthegraphitesurface[24].BothapproachesgreatlyimprovedthecyclingperformanceofLiFePO4cellsat55 C.Anothersolutionwastosigni cantlysuppresstheirondissolu-tionfromtheLiFePO4cathode,forexample,bysubstitutinglithiumbis(oxalato)borate(LiBOB)forLiPF6salt[22,25],orintroducinganadditiveofvinylenecarbonate(VC)(2wt%)intotheelectrolyte[23].

Inthepresentwork,aprismaticLiFePO4-basedcellwithhighcapacity(16.4Ah)isexploredtostudycelldegradationthroughacceleratedcyclingunderatypicalPHEVcondition(highcurrentrateanddeepdepthofdischargeatelevatedtemperature).Thisresearchprovidesanimprovedunderstandingofthedegradationandcyclelifeofhighcapacitybatteryinautomotiveapplications.Thecyclingdegradationwasexaminedthroughcharacterization

第1页