Synthesis and characteristics of Y-zeoliteMCM-48 biporous molecular

74Y.Zhangetal./AppliedCatalysisA:General345(2008)73–79

FT-IRindicatethatthebiporousmaterialpossessesbothpropertiesofMCM-48andzeoliteY-zeolite,butatthesametime,itisdifferentfromeachofthem.ThebiporoussampleshowsstrongeracidstrengthandhigherhydrothermalstabilitythanMCM-48.2.Experimentaldetails

2.1.Preparationofbiporousmaterial

InordertosynthesizeY/MCM-48biporousmolecularsieve,thesolofMCM-48wasprepared rstly.Whilestirring,someamountofNaY(Si/Al=2.4,TheCatalystPlantofNankaiUniversity)wasaddedtothecolloidalprecursorofMCM-48havingthefollowingchemicalcomposition:1TEOS:0.415CTAB:0.48NaOH:55H2O.Thenthemixturewasstirredforabout50minfollowedbythehydrothermalcrystallizationat383Kforaperiodoftime.Aftercoolingtoroomtemperature,theresultingsolidproductwas ltrated,washedthoroughlywithdeionizedwateranddriedbetween373and383K.Then,thecompositemolecularsievesamplewasobtainedbytheproductbeingcalcinedat823Kfor6hintheair.The ltratewastakenouttoprepareforquasi-quantitativeanalysis.TheMCM-48,whichisnamedSi-MCM-48inthisarticle,waspreparedfromtheinitialsolwithoutaddingNaYbythesameapproachabove.ThemechanicalmixturewaspreparedfromthemixingofNaYandMCM-48preparedabove.Thecetyltrimethylammonium(CTA)ion-exchangedY-zeoliteforNH3-TPDstudywaspreparedbydippingNaYzeoliteintheCTABsolutionof30wt.%for24hfollowedby ltration,washingandcalcination.

2.2.Characterization

XRDpatternswerecollectedwithaRigakuD/MAX-PC2200Xdiffractometer(40kV,30mA)usingCuKaradiation(l=0.1541nm).Allsampleswerescannedunderthesameconditions(2u=1–258).Scanningelectronmicrographs(SEM)wererecordedusingaPhilipsXL30SEMtomeasurethespherediametersandtheappearanceoftheparticles.Transmissionelectronmicrographs(TEM)wererecordedonaPhilipsTECNAI20instrumentforcharacterizingtheporesystemofthesamples.Adsorptionanddesorptionisothermsofnitrogenwereobtainedat77KonanAmericanNOVA-2000Sorptometerinstrument.ThelinearpartoftheBrunauer–Emmett–Teller(BET)equationwasusedforthespeci csurfaceareadetermination.Theporesizedistributionswereobtainedfromadsorptionbranchofthenitrogenphysisorp-tionisothermsusingtheDFTmethod.AdditionalspectroscopicinvestigationsofthesampleswereperformedwithFT-IRspectro-scopyonaBrukerTENSOR27FT-IRspectrometeroverwavenumberrangefrom4000to400cmÀ1.Theaciditycharacterizationwasstudiedbyammoniatemperature-programmedmethods(NH3-TPD)onaTP-5000instrument.Thesampleswerepretreatedat550KinHegas(atarateof30mlminÀ1)for1hbeforetheywerecooledtoroomtemperature.Thentheammoniagaswasabsorbedtosaturationbypulseinjectionatroomtemperaturefollowedby ushingthesamplewithHegasfor1htoremovethephysicallyabsorbedmaterial.Thetemperature-programmeddesorptionwasmeasuredwithaTCDdetector.Ammoniadesorptiontemperaturesrangefrom330to773Katarateof4.73K/min.Theanalysisofthe ltratewascarriedoutonaSOLAARM6atomicabsorptionspectrophotometerofAmericanThermoFisherScienti cCorpora-tion.Inordertoevaluatethehydrothermalstabilityofsamplesprepared,thecalcinedcompositesampleandSi-MCM-48werecharacterizedbyXRDafterhavingbeenplacedintheboilingwaterfor1h,respectively.XRDpatternswereobtainedaftertheboiledsampleswere lteredanddriedat383Kfor3h.LossesintheXRD

peakintensity,ascomparedwiththosebeforetheboilingtreatment,wereusedtoevaluatethehydrothermalstabilityofthesamples.

3.Resultanddiscussion3.1.Analysisofstructure

Fig.1istheXRDpatternsofthecompositeswithaddingdifferentamountofNaYandSi-MCM-48.TheaddedNaYcontributeapercentageof5,7and10ofthemassofMCM-48solforcomposite1,composite2andcomposite3,respectively.Itindicatesthatallthecompositesamplesprocessthreedistinctcharacteristic(211),(220)and(420)re ectionscorrespondingtoMCM-48,whichcon rmtheappearanceofcubicmesoporousMCM-48structureinthecompositematerialsand2uofthesere ectionsarealllowerthanthatofSi-MCM-48(Fig.1).Thisphenomenahasalsobeenfoundbyotherresearchers[22]anditshowsthattheunitcellofmesoporousMCM-48phasebecomeslargerafteritiscombinedwithmicroporousY-zeolite.Thismightbeattributedtotheinterfacialeffectbetweenmicro-andmesoporousphase,viz.theactive–OHonthesurfaceofMCM-48isabletocombinewithaluminum(fourcoordinationnumbers)onthesurfaceofY-zeolitetoformSi–O–Alstructure,whichisinfavorofthemorestablecombinationbetweenthetwotypesofmaterialsandthelessshrinkageofthecompositematerialinthecourseofcalcinations.However,itstillneedsadvancedstudytoclarifythephenomena.TheBraggre ectionsinthehigh2uregionfrom5.58to258characteristicofY-zeoliteindicatetheexistenceofstructureofY-zeoliteincompositesample.Beside,italsocanbeseenthatwhenthepercentofaddNaYchangedfrom5%to10%,allthecompositespreparedshowbothwell-structuredMCMmesoporesandY-zeolitemicropores,butthecomparisonamongtheXRDpatternsindicatesthatthecompositewith7%addedNaYrepresentsmorebetterMCM-48structurethanothers,whichshowsthepercentofNaYin uencetheformationofMCM-48.AndallabovepresentthatthestructureofmicroporousY-zeoliteisnotaffectedbyMCM-48formedlaterandthesamplepreparedisacompositematerialcontainingY-zeoliteandMCM-48.

Effectofhydrothermalcrystallizationtimeonthestructureofcomposite2materialcanbeseeninFig.2.Itcanbeenseenthatwiththehydrothermalcrystallizationtimeincreasing,theintensityofMCM-48re ectionsincrease rstlyandreachthehighestvaluewithhydrothermalcrystallizationtimeincreasing

Synthesis and characteristics of Y-zeoliteMCM-48 biporous molecular

of

Fig.1.XRDpatternsofthecompositeswithaddingdifferentpercentageofNaYandSi-MCM-48.