JournalofPowerSources146(2005)

555–558
Formationofimpuritiesonphospho-olivineLiFePO4during
hydrothermalsynthesis
KeisukeShiraishia,b,KaoruDokkoa,b,KiyoshiKanamuraa,b,
a
DepartmentofAppliedChemistry,GraduateSchoolofEngineering,TokyoMetropolitanUniversity,1-1Minami-Ohsawa,
Hachioji,Tokyo192-0397,Japan
bCRESToftheJapanScienceandTechnologyAgency,4-1-8Honcho,Kawaguchi,Saitama332-0012,Japan
Availableonline31May2005
Abstract
Phospho-olivineLiFePO4asacathodematerialofrechargeablelithiumbatterywassynthesizedfromLiOH,FeSO4,and(NH4)3PO4byhydrothermalprocessat170 C.TheoptimizedmolarratioofLi:Fe:Pinthestartingsolutionwas2.5:1:1.Thechargeanddischargecapacitiesat3.5VversusLi/Li+ofhydrothermallysynthesizedLiFePO4were65mAhg 1.Theadditionalheattreatmentwascarriedouttoimprovethecharge–dischargeperformanceofhydrothermallysynthesizedLiFePO4.Ramanspectroscopyrevealedthatexistenceof -Fe2O3ontheparticlesurfaceofLiFePO4annealedat400 C.ThechargeanddischargecapacitiesoftheannealedLiFePO4were150mAhg 1.Twoplateausat3.5and2.5Vwereobservedinthecharge–dischargecurves,andthe2.5VplateauwascorrelatedwiththeLi+insertioninto -Fe2O3.©2005ElsevierB.V.Allrightsreserved.
Keywords:Phospho-olivineLiFePO4;Hydrothermalsynthesis;Rechargeablelithiumbatteries;Cathodematerials;Ramanspectroscopy
1.Introduction
Rechargeablelithiumbatterieshavebeenutilizedinawiderangeofapplications,suchaselectronicdevices.Hightem-peraturebehaviorofarechargeablelithiumbatteryisakeyis-sue,becauseitcanbeheatedinadvertently.However,presentcathodematerials,suchasLixCoO2,aremetastable,andoxy-genevolutionoccursduringdecompositionofLixCoO2atel-evatedtemperatures[1].Ontheotherhand,phospho-olivineLiMPO4(M=Mn,Fe,Co,orNi)havebeenintensivelyinves-tigatedbecauseoftheirhighstability[2].TheyhaveahighlystablethreedimensionalframeworkduetostrongPOcova-lentbondsin(PO4)3 polyanion,whichprohibitsthelibera-tionofoxygen[3].Thesecharacteristicsprovideanexcellentsafetyandastableoperationofbatteryevenunderunusualconditions[4–7].Moreover,LiFePO4isalowcostmaterialandhighlycompatibletoenvironment.
LiFePO4canbesynthesizedbynormalsolid-statereac-tion.Unfortunately,itisverydif culttoachievethetheo-
Correspondingauthor.Tel.:+81426772828;fax:+81426772828.E-mailaddress:kanamura-kiyoshi@c.metro-u.ac.jp(K.Kanamura).
reticalcapacityofLiFePO4,becauseofitslowelectronicconductivityandslowdiffusionofLi-ionintheolivinestructure[3,4,8].Sofar,severalalternativesyntheticmeth-odshavebeenappliedtopreparationofLiFePO4.Recently,ithasbeenreportedthatthecontrolofLiFePO4particlesizeiseffectivetoincreasethechargeanddischargeca-pacities[4].Ithasbeenalsoreportedthathighlydispersedconductivesubstancessuchascarbonaceousmaterialsandsomemetalsinthecathodecompositeelectrodeenhancethecharge–dischargeperformanceofLiFePO4[9–15].Further-more,Chungetal.reportedthatsubstitutionofsmallfractionofFeinLiFePO4byothermetalsincreasestheelectroniccon-ductivityofLiFePO4,anditimprovedthecharge–dischargerateperformanceofLiFePO4[8].
Inthiswork,hydrothermalsynthesiswasemployedforpreparationofphospho-olivineLiFePO4.Thehydrothermalsynthesisisausefulmethodtoprepare neparticles,whichhassomeadvantagessuchassimplesynthesisprocessandlowenergyconsumption.Yangetal.havealreadydemon-stratedthehydrothermalsynthesisofLiFePO4[16].Inthepresentpaper,theoptimizedhydrothermalconditionwasex-ploredtoobtainsinglephaseofLiFePO4.Theadditionalheat
0378-7753/$–seefrontmatter©2005ElsevierB.V.Allrightsreserved.doi:10.1016/j.jpowsour.2005.03.060
Formation of impurities on phospho-olivine LiFePO4 during hydrothermal synthesis [J]. Journal of power Sources, 2008, 146(1/2): 555- 558. 图 6 不同...
of surface impurities on LiFePO4 particles prepared by a hydrothermal process...during decomposition of LixCoO2 at elevated temperatures.1 Phospho-olivine ...
via hydrothermal route_材料科学_工程科技_专业资料...phosphpo-olivine LiFePO4 [13,14], and no ...(PO4 )OH were obtained as impurities due Fig....
Kiyoshi Kanamura. Formation of Impurities on Phospho - olivine LiFePO4 During Hydrothermal Synthesis 〔. Journal of Power Sources, J〕 2005, 555 - 558. ...
Introduction Olivine-type LiFePO4 has been ...mechanochemical activation, and hydrothermal method [...impurities such as Li3PO4, FePO4, Li3Fe2(PO4)...
Synthesis of olivine LiFePO4 cathode materials by mechanical alloying using iron...In our previous work LiFePO4 /C composite compound containing no impurities ...
LiFePO4 is an olivine-type compound, and Li+ ...formation of impurities, the concentration of the ...growth of LiFePO4 during the hydrothermal process....
Among these methods, hydrothermal method offers ...No impurities such as Li3 PO4 , which often ...3.2. Formation mechanism In order to investigate...
LiFePO4 has an orthorhombic olivine structure, in...complexing agents for the formation of the gel. ...detectable impurities such as Li3 PO4 has been ...
olivine; carbon deposition; hydrothermal synthesis 1...formation of LiFePO4 and introducing impurities. The...Phospho-olivines as positive-electrode materials for...