Double-Layered Photoanodes Variable-Size Anatase TiO2 Nanospindles
Table1:StructuralandperformancecharacteristicsofDSSCsbasedonphotoanodesofDSC-1,DSC-2,andDSC-3.DSSC
Voc[mV]755760750
Jsc
[mAcmÀ2]8.416.411.6
FF[%]67.866.866.6
h[%]4.308.325.79
Surfacearea[m2gÀ1]35.176.551.2

Adsorbeddye[ 10À7molcmÀ2]0.891.661.18
DSC-1DSC-2DSC-3
SPfilmis1.49timesthatofthefilmderivedfromP25,andclearlybenefitsfromthehighsurface-to-volumeratioofthesmallnanospindles.TheporesizedistributionsofthethreefilmsdeterminedfromtheirN2absorption/desorptioniso-thermsareshowninFigureS3.TheP25filmshowsanarrowporesizedistributioncenteredat21.0nm,whichsuggeststhattheirregularlyshapednanoparticleswithameangrainsizeofabout25nmarewellorganized(FigureS2b).Whiletheothertwofilmsbothdisplaybroadporesizedistributions(18–80nmforthesinglelayeroflargenanospindles,and11–70nmforthedoublelayerofsmallandlargenanospindles),thedouble-layeredfilmhasanarrowporesizedistributionaround15.8nm,whichclearlyalludestoitsmainoriginfromtheinterstitialvoidsarisingfromtheclosepackingofsmallTiO2nanospindles.ThenarrowaverageporesizestillappearssuitableforDSSCswithabundantdyeadsorption,efficientelectrolytetransport,andhencehighperformance.
Afterdyeloading,cellswithasinglelayeroflargenanospindles(DSC-1),adoublelayerofsmallandlargenanospindles(DSC-2),andP25(DSC-3),weresubjectedtomeasurementsofcurrent–voltage(J–V)characteristicsunderilluminationofAM1.5simulatedsunlightwithapowerdensityof100mWcmÀ2.Figure2showstheJ–Vcurvesof
Figure1.a,b)SEMandTEMimagesoftheas-preparedlargeTiO2nanospindles.c,d)HRTEMimageandthecorrespondingSAED
patternofatypicalnanospindle.e,f)SEMandTEMimagesoftheas-preparedsmallTiO2nanospindles.Cross-sectionalSEMimagesforasinglemesoscopicTiO2layerpreparedfromlargenanospindles(g)andadouble-layerstructurefromlargeandsmallnanospindles(h).Insetofa):EnlargedSEMimageshowingtheclosepackingoflargeTiO2nanospindlebundles.Insetofc):SchematicillustrationoftheanatasecrystalplanesofTiO2nanospindles.Insetoff):EnlargedTEMimageoftheas-preparedsmallTiO2nanospindles.
SmallTiO2nanospindlesobtainedfromaviscouswater/ethyleneglycolsolutionareshowninFigure1eandf.Thewell-definedshape,size(ca.8 20nm),anduniformityofthenanospindlesareclearlyrecognizable.Figure1gandhshowSEMcross-sectionalimagesofasingle-layeredfilm(ca.10.6mmnanospindles)andadouble-layeredstructure(ca.6.1mmnanospindlesandca.4.7mmnanospindles)onfluo-rine-dopedtinoxide(FTO)substrates,respectively.Forcomparison,standardDegussaP25TiO2wasalsousedtoprepareafilmofthesamethicknessbythesamedoctor-bladetechnique(seefilmmorphologyinFigureS2a).TheBruna-uer–Emmett–Teller(BET)surfaceareasofthesefilms(Table1)are35.1(largenanospindles,DSC-1),76.1(double-layerednanospindles,DSC-2),and51.2m2gÀ1(P25,DSC-3),respectively.Thesurfaceareaofthedouble-layered
Figure2.J–VcurvesofDSSCsfabricatedfromthethreeTiO2samplesunderAM1.5Gsimulatedsunlightwithapowerdensityof100mWcmÀ2.&DSC-1;*DSC-2;~DSC-3.
thesesolarcells,andtheresultantphotovoltaicparametersaresummarizedinTable1.Theapproximately10.5mm-thickTiO2photoanodemadeofP25nanoparticlesshowedashort-circuitcurrentdensity(Jsc)of11.6mAcmÀ2,open-circuitvoltage(Voc)of750mV,andfillfactor(FF)of66.6,whichleadtoanoverallenergy-conversionefficiency(h)of5.8%.TheperformanceofDSC-1derivedfromasinglelayerof

large
Angew.Chem.Int.Ed.2010,49,3675–3679
3676doc.guandang.net
2010Wiley-VCHVerlagGmbH&Co.KGaA,Weinheim
509–512 #2008 The Japan Society of Applied Physics Fabrication of Double Layered Hybrid Solar Cells Consisting of Low-Temperature Anatase Titanium Oxide and...
2 “Double-layered Photoanodes from Size-Varied Anatase TiO2 Nanospindles: A Promising Candidate for High Efficiency Dye-Sensitized Solar Cells”. Yongcai ...
509–512 #2008 The Japan Society of Applied Physics Fabrication of Double Layered Hybrid Solar Cells Consisting of Low-Temperature Anatase Titanium Oxide and...