Enhancing Fatigue Performance of Sandwich Composites with Nanophased Core

PU materials

4

Table2:Quasi-staticsheartestresults.

Property

ShearStrength(MPa)

NeatPolyurethaneFoamSandwich

0.550.640.66

Ave.:0.61±0.014

11.711.912.4

Ave.:12.0±0.35

JournalofNanomaterials

ShearModulus(Mpa)

1%CNFPolyurethaneFoamsandwich

0.830.810.78

Ave.:0.81±0.02

13.714.914.4

Ave.:14.3±0.

Enhancing Fatigue Performance of Sandwich Composites with Nanophased Core

32

%Improvement

+33

+19

1

0.8Shearstress(MPa)

0.60.4

3.2.ShearFatigueTests.ShearfatiguetestswereperformedinaccordancetoASTM394-62atroomtemperatureunderloadcontrolonthesandwichspecimensataloadratioofR=|Pmin|/|Pmax|=0.1,usinganMTSmachineatafrequencyof3Hz.Therunoutcyclenumberwassetat106cycles.Fatiguedataforaminimumofthreespecimensineachcategoryofsandwichcompositesweregeneratedatstresslevelsof90%,80%,70%,60%,and50%oftheultimatestaticshearstrength.

3.3.MicroscopicAnalysis.VirginsurfaceswereexaminedinaJEOLJSM5800scanningelectronmicroscope.Thespecimensweregluedtoanaluminumbaseandcoatedwithgoldtopreventchargebuild-upbytheelectronsabsorbedbythespecimen.Microstructuralanalysiswasperformedonbothneatandnanophasedpolyurethanefoams.

0.2

0Shearstrain

Figure4:Stress-Straincurvesforpureandnanophasedfoamsandwich.

4.ResultsandDiscussion

4.1.Quasi-StaticShearTests.Quasi-staticsheartestswereconductedprimarilytoobtainstrengthvaluesforthefatiguetests.LoadwasappliedtotheneatandnanophasedsandwichspecimensviathesteelplatesasshowninFigure3(b).Thelaserdisplacementunitrecordeddisplacementofthemovingsteelplaterelativetothe xedplate.Thisdisplacementwasusedtocalculatetheshearingstrain,γ.Figure4showsrepresentativestress-strain(τ-γ)curvesforneatandnanophasedsandwiches.ShearstrengthofnanophasedfoamasseeninFigure4washigherthanthatofneat.Attheinitialstageofloadingsmallcrackswerenoticedinthecoreneartheedgeofthespecimen.Astheloadingcontinued,thespecimenelongated,smallcrackscoalescedintoadominantcrack,andkinkedintothecore.Crackformationandpropagationwereidenticalwithbothcategoriesoffoams,butelongationwithnanophasedfoamwashigher.Inthenextsequence,rapidshearingofthecoreoccurredandthespecimenfailedatthesub-interfacesectionandalsodiagonallyacrossthethicknessofthecore.Nanophasedfoamcoresandwichdemonstratedmoreductilebehaviorthanneatsandwich.ThisductilityisevidentbythelongersheardeformationregionfornanophasedsandwichseeninFigure4.Thelargedi erenceintheshearelongationclearlydemonstratesthatnanophasedfoamcorehashigherresistancetoshearfailure.

samplestothesteelplates.Theepoxywasallowedtocureatroomtemperatureforaminimumof48hourspriortotesting.The xturewasinstalledinaservohydraulictestingmachine(MTS) ttedwitha100kNloadcellasshowninFigure3(b).Thetestswereconductedatroomtemperatureindisplacementcontrolmodeatacross-headspeedof1.27mm/min.AKeyencelaserdisplacementunitcoupledtoanRD-50Rcontrollerwasinstalled(Figure(3b))tomeasuretheslidingmovementoftheloadingplatesrelativetoeachotherinthedirectionparalleltotheloadingplates.Theshearstress,τ,isgivenby

τ=

P,Lb

(1)

wherePistheloadonthespecimen,Listhelengthofthespecimen,andbisitswidth.Theshearstrain,γ,is

γ=

r,(2)

whereristhedisplacementofoneloadingplatewithrespecttotheotherand,c,denotesthethicknessofthecore.

上一页第4页