2.3 INSTALLATION OF THE FRP REINFORCEMENTS
Figure 2 shows the details of cross-sections of the specimens. The strengthening process of EBR specimen (CPL-50-BOND) was proceeded by the surface treatment using a grinder, followed by the bonding of the CFRP strip. The strengthened beams were cured at ambient temperature for 7 days for the curing of epoxy adhesive. The process for NSM strengthening progressed by cutting the grooves at the bottom of the beams using a grinder, cleaning the debris, and embedding the CFRP strip after application of the adhesive. The

strengthened beams were cured for 3 days so that the epoxy adhesive achieves its design strength.
2.4 LOADING AND MEASUREMENT METHODS
All specimens were subjected to 4-point bending tests to failure by means of UTM (Universal Testing Machine) with capacity of 980 kN. The loading was applied under displacement control at a speed of 0.02 mm/sec until the first 15 mm and 0.05 mm/sec from 15 mm until failure. The measurement of alltest data was recorded by a static data logger and a computer at intervals of 1 second. Electrical resistance strain gauges were fixed at mid-span and L/4 to measure the strain of steel reinforcements.Strain gauges to measure the strain of concrete were located at the top, 5 cm and 10 cm away from the top on one side at mid-span. Strain gauges were also placed on the FRP reinforcement located at the bottom of the mid-span and loaded points to measure the strain according to the loading process.
3. EXPERIMENTAL RESULTS
3.1 FAILURE MODES
Before cracking, all the strengthened specimens exhibited bending behavior similar to the unstrengthened specimen. This shows that the CFRP reinforcement is unable to contribute to the increase of the stiffness and strength in the elastic domain. However, after cracking, the

of mixes M1, M2 and M3 has increased in strength 114% for M1 mix, 109% for M2 mix and 111% for M3 mix for 6 hours duration of exposure....
建筑土木论文中英翻译 12页 5财富值 土木建筑工程毕业设计论文... 144页 5财富...(cm) Number of stories 9 8 7 6 5 4 3 2 1 SchemeⅠ 0.890 0.812...
译 文 学专学姓 院: 业: 号: 名: 船舶与建筑工程 土木工程 0745512126 肖...图形 6:第二组的 τ-R 骨架曲线 6 江苏科技大学本科毕业设计(论文) 表3 ...
建筑外文文献(含中文翻译... 20页 免费 毕业设计论文致谢词 2页 免费 土木工程...这个循环系统完 6 美了自身, 无论是上升的还是下降的都使其具有优美的形式。...
土木专业毕业设计外文翻... 6页 2下载券 土木工程毕业设计 外文翻... 17页...张辰祺外文翻译 13页 7下载券 建筑施工混凝土裂缝的预... 16页 免费土...
土木工程毕业设计外文翻译_建筑/土木_工程科技_专业资料。土木工程毕业设计外文翻译...与理论的比较 对预应力混凝土框架结构的主要理论预测曲线绘制在图 5 和 6 中。...
土木工程建筑工程毕业设... 22页 2下载券 土木工程(管理)毕业设计... 28页...外文资料翻译 第 6页 Although the length of the latter train doubles that ...
土木工程(管理)毕业设计外文翻译_建筑/土木_工程科技_专业资料。土木工程(管理)...6 RENTAL COSTS If a project is a long distance from the contractor's ...
土木工程毕业设计外文翻译最终中英文_建筑/土木_工程科技_专业资料。7 Rigid-Frame...6. Computer analysis of total structure for more accurate check on member ...
2010011424 指导教师: 张鑫 刘清阳 翻译日期:2014/6/14 山东建筑大学毕业设计外文文献及译文 Concrete Wikipedia This article is about the construction material. ...
热门文档