JournalofMaterialsProcessingTechnology74(1998)23–26
StudyofthethermalfatiguecrackinitiallifeofH13
andH21steels
GuobinLi*,XiangzhiLi,JianjunWu
DepartmentofMaterialScienceandEngineering,HebeiUni6ersityofTechnology,P.O.Box548,Tianjin300132,People’sRepublicofChina
Received13October1996
Abstract
Thispaperhasde nedthethermalfatiguecrackinitial(TFCI)lifefromtheviewpointofengineering.Accordingtothemodi edManson–Cof nexpressionandthestrainrangecausedbythermalstress,anewexpression:Ni=K(DT DTo) 2isderivedtodescribetheTFCIlife.WhenthetemperaturedifferenceDTofthethermalcyclesislessthanthecriticaltemperaturedifferenceDTooftheTFCIlife,i.e.DTBDTo,theTFCIlifeofahot-workdietendstoin nity.ThisstudyalsoshowsthattheDToofH13andH21steelsarerespectively476and436°Cundertheoptimumheattreatmentconditions.H13steelhasabetterthermalfatigueresistancethanthatofH21steel.©1998ElsevierScienceS.A.
Keywords:H13steel;H21steel;Thermalfatiguecrackinitiallife
1.Introduction
H21(3Cr2W8V)steelpossesseshighhotstrengthandthermostability,goodcastability,forgeabilityandcutability,anditiseasilyheat-treatable.InChina,3Cr2W8Vsteelhasbeenappliedwidelytoproducemanykindsofhot-workdies,suchasforthehot-press-ing,hot-extrusionanddie-castingofnon-ferrousmetals.Despitethatthissteelhasbeenreplacedinsomeothernations[1],inChinatungstenhot-workdiesteelisstillofgreatuse.
Internationally,H13(4Cr5MoSiV1)steelisahighhot-strengthchromiumhot-workdiesteelusedwidely.Byvirtueofitshighhardenability,highstrength,hightoughnessandhighthermalfatigueresistance[2],ithasbeenbroughtintotheChinesenationalstandardre-centlyanditsusehasbeenextendedenergeticallywithgoodresult[1,3–6].
Inpracticaluse,H21steelhasahigherhotstrengthandthermostability,butlowerthermalfatigueresis-tance,thanthoseofH13steel[1,7].Forhot-workdiesteel,therearetwomainfailureforms,onebeingwearandtheotherthermalfatigue.Practicallyspeaking,theearlyfractureofahot-workdiecausedbythermal
*Correspondingauthor.
0924-0136/98/$19.00©1998ElsevierScienceS.A.Allrightsreserved.PIIS0924-0136(97)00244-6
fatigueisthemainfailureform[8].Therefore,howtoincreasethethermalfatigueresistanceofhot-workdiesteelhasbecomeoneoftheresearchtopicsofmostconcerntodieworkers[9].
Thepresentauthorshavestudiedthethermalfatiguecrackinitial(TFCI)life(resistance)ofH21andH13steelsunderdifferentheat-treatmentconditionsandhavederivedanexpressiontodescribetheTFCIlife.Inengineering,thisexpressioncanbeusedtopredicttheTFCIlifeofhot-workdiesteeleffectivelyandtopre-venttheearlyfailureofdiescausedbythermalfatigue.2.Testprocedures
2.1.Materialsandspecimenpreparation
2.1.1.Chemicalcompositionofthetestmaterials
ThechemicalcompositionoftestmaterialsisshowninTable1.
2.1.2.Preparationofthespecimens
Afterforgingandannealing,thetestmaterialsweremachinedintospecimensaccordingtothesizesshowninFig.1,wherethenotchof0.35mm×1.8mmwascutafterheat-treatmentby 0.35mmmolybdenumwire.
study presents a methodology of life prediction of fatigue crack initiation ...secondary hardening was observed during most of life after the initial ...
study of the EIFS technique for fatigue design_...Measurements of fatigue crack growth rates on ...Equivalent initial aw size distributions (EIFSD) ...
Thermal fatigue behavior of niobium microalloyed H13 steel_专业资料。维普... Crack growth behavior ... 6人阅读 5页 2.00 Thermal Fatigue Behavi....
Fatigue life prediction based on crack propagation...crack to grow from an initial size to the ...The present study is based on a limited set of...
Effects of pitting corrosion on fatigue life of aluminum alloy Y 12CZ based on initial disconti_专业资料。维普资讯 http://www.cqvip.com Avibl niea ...
improve the fatigue performance of metallic ...During the initial period of exposure, the ...The purpose of this paper is to study the ...
This study aims at elucidating the life-limiting ...The thermal fatigue crack initiation is associated ...of a low-cycle fatigue process.The initial ...
experimentofhotdipaluminizinghadbeencarriedoutinordertostudythe interaction between ...H13diecastingdie,soldering,thermalfatigue,Siand K/Na,Momultiple modification,...
Fatigue-properties-of-rolled-magnesium-alloy-(AZ31... a high thermal conductivity and a high damping ...initial stage, the decrease of the friction force...
fatigue life prediction, the number of cycles ...with the initial crack defined for by the user;... Study of the fatigue l... 9页 1下载券 ...