R.Akhteretal./MaterialsScienceandEngineeringA 447 (2007) 192–196

193
Fig.1.Con gurationoftwinspots.
withthetwinspotsorientatedinlinewithweldingdirection.Thecentre-to-centredistancebetweenthetwinspotswas0.49mm.Thespotcon gurationisshowninFig.1.Theuseofdualbeamconditionsensuresalargerweldpool,facilitatestheporosity’sejectionandstabilizesthekeyholeascomparedwithsinglebeamcon gurations.
Foreachweldthespecimenwasclampedona xedtableandthefocusedbeamwasmovedoverthesheet.Ashieldinggasmixtureofargonandheliumintheratioof2:1wasusedduringtheweldingprocess.Thisprovidedaninertshieldoverthehotreactiveweld.Thegas owratewas20l/min.Heliumisconsideredtobeagoodshieldinggasinlaserweldingbecausehighionisationpotentialoffersresistancetotheformationofplasma.Heliumishoweverlighterthanairandsubstantial owratesarerequiredtoproduceadequateshielding.Argonontheotherhandisheavierthanairandprovidesbettershielding.Itishowevermorepronetoplasmaformationandbecauseitismuchheavierthanheliumittransfersmoremomentumtotheweldpool.Inthecaseofaluminiumtheweldmetalhaslowviscosityandiseasilydisturbed.Webelievedthatamixtureofheliumandargonwouldstrikeanoptimumcompromisebetweentherequirementsofplasmaprevention,shieldingandthesensitivityofthelowviscositymeltpooltomechanicaldisturbance.
Theweldingspeedwasvariedforeachexperimentalweld.Aftertheweldingprocess,theweldedspecimenweresectioned,groundandpolished.TheweldmicrostructurewasobservedbyopticalmicroscopyafteretchingwithKeller’ssolution.X-rayanalyseswerealsoperformedthroughoutthelengthoftheweldtoinvestigatethepresenceofporosities.Amicro-hardnesstesterwasusedtomeasurethehardness.ThetensiletestswereperformedonaLloydM100Kmachine.3.Heattreatment
ToobtaintheT6heattreatmentcondition,theascastandweldedsamplesweresolutiontreatedat540 Cfor6handthenwaterquenchedbeforearti ciallyagedat160 Cfor6h.4.Resultsanddiscussions4.1.Laserwelding
LaserweldingoftheSSMA356aluminiumalloywasper-formed.Arangeofweldingparameterswasusedforthebeadonplatewelding.Fig.2showstherelationshipbetweenweldingspeedanddepth/widthoftheweldinSSMaluminium.

Generally
Fig.2.Weldingspeedvs.depth/widthforweldingSSMaluminiumA356,laserpower4kW,sheetthickness4.2mm,spotseparation0.49mm.
thedepthandwidthdecreasesastheweldingspeedisincreased.Itiscustomarytode nethewidthoftheweldasthewidestpartoftheweldmetal.Thisnormallyoccursattheweldface,i.e.topsurfaceofthesubstrate.Itisgenerallyacceptedthatthewidthoftheweldincreasesastheheatinputincreases.Thisisoftenthecasewhentheavailablelaserpowerisnotquitesuf cienttogivetherequiredpenetrationandspeedhastobereducedinordertoensurefullpenetration.Webelievethatthisisthereasonfortherelativelywidewelds.Becauseofthefactthata600- m brewasusedthepowerdensitywastoolowforfullpenetrationathighspeed.Fullpenetrationcouldonlybeobtainedataspeedthatcorrespondedtoaheatinputthatwastoohigh.Fig.3showsaweldpro lemadebyjoiningtwosheetsinbuttcon gurationusingoptimalparameters.
ThecompositionofthebaseandweldmetalsaregiveninTable1.Itcanbeseenthatthereisnotasigni cantchangeinthecompositionafterwelding.4.2.Microstructure
Themicrostructureoftheascast(F)basemetalandweldfusionzoneisshowninFig.4aandb.Themicrostructureof

the
Fig.3.Weldpro leofaluminiumalloyinbuttcon guration:laserpower,3.8kW;speed,1.92m/min;spotseparation,0.49mm;sheetthickness,4.0mm.
The effect of microstructure on the mechanical properties of two-phase titanium...b titanium alloys after different heat treatment. The in?uence of the ...
Effect of post-weld heat treatment on microstructure and properties of Ti-23Al-17Nb alloy laser_专业资料。Available online at、^『、『讥Ⅳ.sciencedirect...
2.Effect of heat treatme... 7页 2财富值 Effect of pre post T6 he.....Effect of heat treatment on mechanical properties of hazelnut wood (Corylus ...
EFFECT OF OF HEAT TREATMENT CAST IRON ON THE PROPERTIES HIGH-CHROMIUM M. ...The mechanical properties are highest after normalization at 1200 o . C ...
, 2014, 27(2), 245–252 DOI 10.1007/s40195-014-0052-4 Effects of Post-Weld Heat Treatment on Microstructure and Mechanical Properties of Al-12.7Si...
Effect of Temperature on the Mechanical Properties of Polymer Mortars_物理_自然科学_专业资料。Materials Research. 2012; 15(4): 645-649 DOI: 10.1590/S15...
Effect of Pre-oxidation on the Properties of Crushed Bituminous Coal and Activated Carbon Prepar_专业资料。维普资讯 http://www.cqvip.com De.07c2o JunlfChn...
Effect of pre post T6 ... 5页 1下载券 Effects...transglutaminase treatment on the properties of cast...on the mechanical and barrier properties of soy ...
Effect of pre-deformation on aging characteristics...mechanical properties of Mg-Gd-Nd-Zr all_专业...Effect of DH treatment... 1人阅读 6页 2....
Effect of heat treatment... 暂无评价 4页 2.00...Effect of pre post T6 he... 5页 1财富值喜欢...Heat storage effect of mechanical properties of ...
热门文档