Quality improvements by use of FC Mold
on hot rolled coils
Hongliang Yang*, Jingxin Song**, Nils Jacobson*, Olof Sjöden*, Jan-Erik Eriksson*, Helmut Hackl*
*ABB AB/Metallurgy Västerås, Sweden
E-mail: Hongliang.yang@se.abb.com ** Meishan Steelworks, Baosteel group, China Abstract: The effects of FC Mold in a slab caster mold are studied by inspecting the surface quality of hot rolled coils. A defect index is proposed to represent the casting-related defects of hot rolled coils. FC Mold improves the coils’ surface quality by up to 60% depending on the casting parameters and FC Mold operations. A dimensionless mold index () is proposed to unite the casting parameters such as casting speed, throughput, slab width and thickness, and it is found that the mold index can be the controlling parameter in determining the FC Mold effects. It is also found that the magnetic interaction number () can be used to optimize the operation of FC Mold under different casting conditions. Both numerical and water model simulations are carried out to study the influence of the FC Mold on the flow field in the mold. Both types of simulations show that the jet flow from the SEN turns into a horizontal flow when it comes into contact with the DC magnetic field. The jet flow momentum, DC magnetic field strength and length of the horizontal flow will determine the braking effect of DC magnetic field in total. The findings from the simulations also justify the use of mold index and magnetic interaction number. Key words: FC Mold, Mold index, Magnetic interaction number
confirmed by checking the inclined angle of the dendrites at the narrow face [1]. The increase of the

outlets of SEN [1].Due to the increase of meniscus temperature and stabilization of meniscus fluctuations by the static magnetic field, the variation of the pitch and depth of oscillation marks on middle carbon steel are reduced, as well as the frequency of longitudinal cracks.[2] The quantity of inclusions in the slab subsurface area is effectively reduced because of the reduced penetration depth.[3] D. van der Plas et. al [4] have made plant trials investigating the influence of EMBR Ruler on slab cleanliness and final product quality. It was found that EMBR Ruler can reduce the rejection ratio on critical steel grades up to 50% after cold rolling, and that EMBR performance is affected by casting parameters as mold width, casting speed and argon flow rate. H. Yamamura et. al [5] have studied the influence of magnetic flux density on the flow patterns by analyzing solid structures and numerical simulations. The magnetic interaction number was proposed to correlate the casting conditions and the quantity of inclusions in the as-cast slabs. Y. Miki and S. Takeuchi [6] have made slab analyses and LES simulations and found that bubbles and inclusions can penetrate deeply into the slabs due to asymmetric unbalanced flow in the mold, and FC Mold can reduce the time dependent flow and thereby prevent the internal defects caused by
bubbles and inclusions.
In this paper, as a continuation of the previous paper [7], steel plant measurements on the influence of FC Mold on the hot rolled coils quality were presented.
) and Two dimensionless numbers, mold index (
magnetic interaction number () were employed to
1. Introduction
FC Mold, an electromagneticflow control technology in the slab caster mold, has been widely installed worldwide since the 1990s. The FC Mold uses two static magnetic fields, an upper field at the slab meniscus level to control the meniscus metal flow velocity and a second independently controlled lower field in the lower part of the mold to minimize the penetration depth of the steel jets from the SEN, see Fig.1. EMBR Ruler is an earlier generation of FC Mold with only one level static magnetic field. JFE Steel was the first company to publish the results of static magnetic field on as-cast slabs. Reduction of the penetration depth by static magnetic field was
炉渣) 包钢罩式退火用的燃料为煤气,排废合理运用。... RH真空处 理装置 连 结晶器 铸机 钢坯 热轧 ?...只能通过不断的 改进设备,提高工艺,以达到最小的...
ECCC-42结晶器显示屏,一种... ECCC-43小方坯连铸上初始凝... ECCC-50从... ECCC-193通过数学和统计的... 7页 免费 武钢二热轧板坯库实时生产... 7页...
保护渣要求使用专用保护渣,结晶器喂铝线(或稀土铝...5、产品应用及质量改进带钢经用户冷轧成 0.9×31....特别适用于各大钢厂的热轧卷 板、冷轧卷板自动打包...
热轧卷表面夹杂缺陷的分析与控制_专业资料。对低碳热轧卷表面夹杂缺陷形貌、分布规律及相应成分进行分析。结果表明,结晶器保护渣卷入是引起低碳热轧卷表面夹杂缺陷的...
保护渣要求使用专用保护渣,结晶器喂铝线(或稀土铝...5、产品应用及质量改进带钢经用户冷轧成 0.9×31....特别适用于各大钢厂的热轧卷 板、冷轧卷板自动打包...
热门文档