PNIPAM-Modi edPorousSilicaNanoparticlesahydratedtoadehydratedstate17,18)of~32°Cinwater.19Thus,attemperaturesbelowtheLCST,thepolymerisinthecoil(soluble)conformation,whileabovetheLCST,itisintheglobuleorcollapsed(insoluble)state.Thispropertyhasbeenexploitedinapplicationsrangingwidelyfromrheologymodi cationstodrugdelivery.20,21
Studiesonmesoporoussilica-PNIPAMhybridsarefew.Lo´pezandco-workerspreparedhybridsbyeitherconductingatomtransferradicalpolymerization(ATRP)oftheNIPAMmonomerfromthesurfaceofcalcinedMCM-41treatedwithaninitiatororcogelationofanaminopropylsilyl-terminatedPNIPAMwithsilicainthepresenceofasurfactanttemplate.22,23Bothmethodsproducematerialscapableof uoresceinuptakeandreleaseabovetheLCSTofPNIPAM(40-50°C),andthelattermethodproducedmembranescapableofrejectingcrystalvioletatlowtemperatures.ThedataareconsistentwithamechanismwherebythepolymersareencapsulatedwithintheporesofMCM-41,actingtoreducesmallmoleculediffusionwhenintheopencoilcon gurationwhilefacilitatingdiffusionintheglobuleconformationbyeffectivelyretreatingtotheporewalls.However,thesesystemsareveryleakyatroomtemperature,releasingone-halftoone-thirdofthequantityof uoresceinreleasedat40-50°Cafterjust2h,andtheparticlesareverylarge(10-20µm)andthuspoorlydispersible.22,23Herein,wepresentPNIPAM-modi edmicro-to-meso-poroussilicananoparticles(MSN)withsizesontheorderof100nmpreparedbychemicalattachmentofpreformedpolymertoprepreparedporousparticles.Importantly,thesenewmaterialsshowminimalleakageinthe“closed”conformation(<2%releaseover2hvs>25%releaseintheLo´pezsystem22).Theseimprovementsappeartoberelatedtoadifferentmodeofactionthanseenpreviouslysincetheuptakeandreleaseinthepresentlyreportedsystemoccursabove,ratherthanbelow,theLCST.
ExperimentalSection
Materials.Tetraethylorthosilicate(TEOS),3-mercaptopropyl-trimethoxysilane(MPTMS),N-cetyltrimethylammoniumbromide(CTAB),5,5′-dithiobis-2-nitrobenzoicacid(Ellman’sreagent),N-isopropylacrylamide(NIPAM),2,2′-azobisisobutyronitrile(AIBN),and2,2′-dipyridyldisul de(Aldrithiol-2)wereallpurchasedfromAldrichandusedasreceived.NanopurewaterwasdispensedfromaNanopureDiamond,Barnsteadpuri cationsystem.
Synthesisof2-Dodecylsulfanylthiocarbonylsulfanyl-2-methylPropionicAcid(DMP).1-Dodecanethiol(20.2g,0.10mol),acetone(58.0g,1.0mol),andtricaprylylmethylammoniumchloride(1.0g,0.0025mol)wereaddedintoa askandcooledto0°Cunderanitrogenatmosphere.Sodiumhydroxidesolution(50%)(9.0g,0.11mol)wasaddedoveraperiodof10min.Afterthe
(17)delasHerasAlarco´n,C.;Pennadam,S.;Alexander,C.Chem.Soc.
ReV.2005,34,276–285.
(18)Yerushalmi,R.;Scherz,A.;vanderBoom,M.E.;Kraatz,H.-B.J.
Mater.Chem.2005,15,4480–4487.
(19)You,Y.-Z.;Hong,C.-Y.;Pan,C.-Y.;Wang,P.-H.AdV.Mater.2004,
16,1953–1957.
(20)Qiu,Y.;Park,K.AdV.DrugDeliVeryReV.2001,53,321–339.(21)Kopecek,J.Eur.J.Pharm.Sci.2003,20,1–16.
(22)Fu,Q.;Rao,G.V.R.;Ista,L.K.;Wu,Y.;Andrzejewski,B.P.;Sklar,
L.A.;Ward,T.L.;Lo´pez,G.P.AdV.Mater.2003,15,1262–1266.(23)Fu,Q.;Rao,G.V.R.;Ward,T.L.;Lu,Y.;Lo´pez,G.P.Langmuir
2007,23,170–174.
Chem.Mater.,Vol.20,No.10,20083355
Scheme1.SynthesisofPyridylDisul de-Terminated

PNIPAM
mixturewasstirredforanadditional20min,carbondisul de(7.6g,0.10mol)inacetone(10.0g)wasaddedover30min,andthecolorturnedgraduallyred.Chloroform(17.8g,0.15mol)wasadded,followedbydropwiseadditionof40gof50%sodiumhydroxidesolutionover20min.Themixturewasstirredovernight;then200mLofwaterwasadded,followedby80mLofconcentratedHCltoacidifytheaqueoussolution.Afterremovingorganicsolvents,thesolidwas lteredandthenstirredin300mLofisopropanol.Theinsolublesolidwas lteredoff,leavinganisopropanolsolutionwhichwasconcentrated,andtheresultingsolidrecrystallizedfromhexanetoafford12.0gofproduct(yield33%).1
HNMRdata:CDCl3(δ)0.89(t,3H,-C11CH23CH3),1.2-1.47(m,18H,-CH2CH2C9H18CH3),1.68(m,2H,-S-CH2CH2-C10H21),1.73(s,6H,-S-C(CH3)2COOH),3.3(t,2H,-S-CH2-C11H23),SupportingInformation,FigureS1.
RAFTPolymerizationofNIPAMToProducePNIPAM-S-C-S)-S-C12H25.Thetemperature-responsivepolymer,PNI-PAM,containingapyridyldisul deendgroupwaspreparedviareversibleadditionfragmentationchaintransfer(RAFT)polymer-izationin3steps(Scheme1).Polymerizationof4.0gofNIPAMwith120.0mgofDMPwasconductedinthepresenceof4.0mgofAIBNin5.0mLofDMFina20mLvial.Thevialwassealedandimmersedinapreheatedwaterbathat60°C.Polymerizationwashaltedbyimmediateexposuretoairandcoolingwithdryice.Theproductwasprecipitatedinether, ltered,anddriedatroomtemperature.PNIPAM-S-C(S)-S-C12H25wascharacterizedus-ingacombinationofsizeexclusionchromatography(SEC)andgelpermeationchromatography.
AminolysisofTrithiocarbonate-TerminatedPNIPAMToYieldThiol-TerminatedPNIPAM.Thetrithiocarbonate-termi-natedPNIPAM(PNIPAM-S-C(S)-S-C12H25)wastreatedwithhexylaminetoyieldthiol-terminatedPNIPAM(PNIPAM-SH)asfollows.A3.0gamountoftrithiocarbonate-terminatedPNIPAMin5mLofDMFwasdeoxygenatedbyastreamofnitrogenfor2h.Tothatsolution,5dropsofNa2S2O4solutionwasaddedtopreventoxidationofthethiolstodisul des.Thiswasfollowedbyadditionof2.0mLofhexylamine.Themixturewasstirredatroomtemperatureforanother12h.Thethiol-terminatedPNIPAM(PNIPAM-SH)wasobtainedbypouringthemixtureintoetherand lteringanddryinginvacuumatroomtemperature.Thetrithio-carbonateabsorbanceat310nmwasabsentfromtheUVspectrumofPNIPAM-SH(SupportingInformation,FigureS2),consistentwithconversionoftrithiocabonategroupstothiolgroups.
PreparationofDisul dePyridyl-TerminatedPNIPAM.Asolutioncontaining2.5gofAldrithiol-2,1.0mLofglacialaceticacid,and20mLofmethanolwasaddedtoa100mLround-bottom askwithstirbar,followedbyadditionofPNIPAM-SH.After24hatroomtemperature,thereactionmixturewasconcentratedunder
多孔硅/硅结构的微观形貌、 纳米力学及温敏特性杨...性 . 测量所得不 同电流密度条件下制备的多孔硅...硅颗粒和孔洞组成的多孔硅基底表面生长行为不同 于在...
纳米力学及温敏特性 氧化钒/多孔硅/硅结构的微观...为了在电性 能测试中电源的两个电极与 VOx 电阻间...薄膜在尺寸为几十纳米 硅颗粒和孔洞组成的多孔硅基底...
性也随 之下降. 关键词: 氧化 钒; 多孑 硅;微观结构;纳米 力学 :温敏 ...膜 在尺 寸 为几 十 纳米 薄 硅颗粒 和孔洞 组成 的多孔硅 基底 表面生 ...
三维网状结构的硅 壳包裹罗丹明 B, 制备出具有核壳结构的纳米颗粒, 接着用...1 温敏性荧光纳米颗粒的红外光谱图 IR spectra of thermosensitive fluorescene ...
三维网状结构的硅壳包裹罗丹明 B, 制备具有核壳结构的纳米 颗粒, 用甲基丙烯...结果与讨论 2.1 温敏性荧光纳米颗粒的表征 对合成的温敏性荧光纳米颗粒进行了...
将分子印迹温敏性水凝胶与多孔硅结合,发展基于多孔硅的分子印迹温敏水凝胶芯片传感器罗乔慧,邬建敏* 浙江大学化学系,微分析系统研究所,杭州,310058? *wjm-st1@...
温敏性PNIPAAm多孔水凝胶制备方法的研究进展_专业资料。聚N-异丙基丙烯酰胺(PNIPAAm)水凝胶由于其大分子侧链上同时含有亲水性的酰胺基和疏水性的异丙基而成为一种典...
多孔温敏凝胶的制备及性能测试_专业资料。N-异丙基丙烯酰胺(NIPA)具有优良的温...温敏性PNIPAAm多孔水凝胶... 74人阅读 5页 2.00 纳米银温敏凝胶的制备...
冷冻多孔温敏凝胶的制备与性能研究_专业资料。以聚乙二醇2000为致孔剂,采用冷冻法合成了聚(N-异丙基丙烯酰胺-co-伊丙烯酰胺)温敏凝胶。结果表明,PEG2000作为致孔...
得到 A ( A *%7 /* : /$ #E 7R/* 7 $ # 纳米级复合材料"由于这种 ? #E 7R/* 7 $ # 纳米级颗粒材料在保持温敏性的 A ( A *%7 /* : /...
热门文档