EffectsofCodopedVC/Cr3C2onMicrostructureand
PropertiesofUltrafineCementedCarbides
LeiYiwenl,Sun
Ronglul,Wu
Enxi2,TangYin91
(1.TianjinPolytechnicUniversity,Tianjin3∞160,Clmla)
(2.StateKeyLaboratoryofPowderMetallurgy,CentralSouthUniversity,Changsha410083,Chi衄)
Abstract:Hardness,R'811BV朗'SCinvestigated.Theresultsshowproportionsintered
at
rupture
s概gth
fiRS)andmicromucUa髓of
that
alloyswithhomogeneousmicrostructare
and麟Hent
WC
VC。Cr3C2codopedultrafineWC-12Cowerewhenoptimal
propertieswcreobtained
ofadditiousw鹋added.TheTRsandhardnessreach3786MPaand91.7HRAforthealloywithO.5%Cr3C2,'O.2%VCand
1430℃.VCismoreeffective
at
conlrollingcontinuousand
discontinuous耐ngrowththanCr3C2,aadtheeffectivenessof
grin
growthinhibitionisthatVC
additionsismoresignificantathighersinteringtemperature.Themechanismofreduceretard
of
the唧ULration
andCr3C2
WCinthebinderphase,decreasethedrivingforceforWCgraingrowthfromreprecipitationprocessand
WCgringrowth.
Keywords:c君mented
carbides;microstmcture;grin
growtll:mechanism
Article
CI£number:TFl25.3Documentcode:A
ID:1002.185X(2009)S1.229-05
Cementedcarbides,whichconsistofhomogeneousdistributionoff-acetedWCgrainsembeddedinbinde!r,a∞typicallyused
as
a
VC/Cr3C2alwayshavehi【ghermechanicalpropertiesthanthosewiththe
sallle
Co-basedcontentofVC
or
Cr3C2.respectivelyIjJ.
drilling
or
cuttingtoolsandInordertoenhancethepropertiesofWC-Co
cemented
wearresistanttoolsbecauseoftheirexcellenthardnessandstrength.Enhancingthestrengthand
carbides,VC/Cr3C2werecodopedinwc-Cocemented
carbidesininhibitors
on
our
hardnessofWC-Coc[18e.Theeffectof
codopedVC/Cr3C2
cemented
withthefacturingmethod
carbideshasbeen
an
importantproblemalong
themechanicalproperties.theWrCgrainsize
developmentofscienceandtechnology.Mallu-cementedcarbides嘶t11finegrinsizeisa900d
to
anditsdistribution,whichareimportantparametersusedas
descriptionsofgradesandasanalyzed.111emechanism
a
relationbetweenphysical
improve
the
properties
ofWC.Cofrom
alloys.
Co
propertiesandmicrostructureincementedcarbides,was
of
codoped
grain
growth
inhibitortoretardtheWCgraingrowthduringthesintering
Cementedcarbides
a心processed
L“.Such
WCand
powdersbyliquidphasesinteringprocessinwhichWCgraingrowthcanis
occur
a
microstructureevolution
processwasalsoaddressedinthiswork.
detrimental
tothe
properties
and
call
belimited
bv
additionofsometransitionmetalcarbidessuch触VC.
1
Experimental
Cr3C2,Ⅻ)C,TaCand
Each
inhibitor
theirmixturesthatinhibit
grain
The
various
carbideswithobtained
grin
sizerangingfrom0.4to0.7
Xiamen
CoLtd.11圮
growthduringthesinteringprocessl2J.
has
its
OWll
岫,were
advantages
and
fromHeron
compositionsofW℃.12CoalloyswithVCand
iar
a
disadvantages■VCismoreeriectiveininhibitingWC
graingrowthandthealloyswittlVCexhibitsufficientlyhigherhardnessthanthosewithCr3C2,butthedrawbackisthat
VC
mayreducethe
toughness
and
the
oxidation
Cr3C2forthisstudywereshowninTab.1.
Powdermixtureswe聘milledfor72h,using
a
lined
wittl
WC-Co
alloyand
WC.Co
balls.Driedin
vaguBm
ovenandthengranulated.111isgranulate
resistanceofthealloysatelevatedtemperature.Althoughthe
Cr3C2is
a
pressed
lesspotentgraingrowthinhibitor,small
a
×43.5衄onBPP—E
intorectangularbarswithsizeof
6.3衄×6.3
was
mm
hydrostaticmachineatthepressure
addition
corrosion
ofCr3C2isresistant
standardwaytoprovidefinegrained
alloyst4捌.Thealloys
with
of200~口a.Greencompacts
we旭debinded.aadthen
WC-Cosinteredat1410.1430and1450℃for1hinGCAfulmace.
Receiveddate:2008.0601
Foundationitem:SupportedbytheUniversityBiography:LeiYiwen,Ph.D.,Lecturer,Schoolof
ScienceandTechniqueDevelopmentFoundationofTianjin(20060912)
MechanicalandElectronicEngineering,TianjinPolytechnicUniversity,T'majin300160。P.1L
China,Tel:008922—89525883,Bmail:leiyiwen@163.corn
万方数据
比例 复合 添加的方式,系统研究 了VC和C 32r 晶粒长大抑制剂总含量为08C. %条件下,V和 C C32 同添加比例对WC1%C 超细硬质合金力学性能及组织结构的影响。...
抑制剂对超细硬质合金组织... 3页 2财富值 淬火...2005 2005 年 12 月 添加剂对硬质合金性能的影响...VC 削性能 ,在合金中添加少量的 TaC 可提高合金的...
显微组织及力学性能的影响, 并结合试验结果分析了超细硬质合金中 VC / Cr3 C2 晶粒长大抑制剂的作 添加适量 VC / Cr3 C2 晶粒长大抑制剂的超细硬质合金中 ...
方式、添加量对 wC.12%Co超细硬质合金性能的影响。按正交试验方法,设计了添 加VC/Cr、C:及(TaNb)...超细硬质合金孔隙度低(‰2),无脱碳相或游离碳组织...
μm不同粒度级别的钴粉,按YF06合金牌号配料,从压坯压力、压坯中钴粉分布以及合金的物理性能和金相组织结构等方面探讨了钴粉粒度对超细硬质合金性能及结构的影响。...
超细晶硬质合金中VC/Cr3C2对晶粒长大的抑制作用及机理研究_专业资料。研究了超细晶硬质合金VC/Cr3C2抑制剂作用及抑制机理。研究发现复合添加VC/Cr3C2可以有效抑制...
超细硬质合金晶粒生长抑制剂VC、Cr3C2作用机理的研究_专业资料。本文以液相复合-连续还原碳化方法制备的掺杂有VC和Cr3C2抑制剂的纳米复合WC-10Co粉末为原料,采用...
超细及纳米硬质合金中碳含量的变化及对组织性能的影响_自然科学_专业资料。硬质合金超细及纳米硬质合金中碳含量的变化及对组织性能的影响/ 张梅琳等 ?65 ? 摘要...
2 0 1 0 # 材料与应用 # 添加金属 Mo 对 WC -Co 硬质合金组织 和性能的影响王丽利, 李海艳, 刘宁 ( 合肥工业大学材料科学与工 程学院 , 安徽 合肥 ...
预处理工艺对放电等离子烧结超细晶WC-Co硬质合金组织和性能的影响_专业资料。采用不同粒度的WC粉与超细Co粉混合得到初始粉末,利用直接放电等离子烧结(SPS)技术和一...
热门文档