本文采用放电等离子烧结的方法制备了纳米石墨烯增强的羟基磷灰石,并和碳纳米管增强的羟基磷灰石作了对比,研究发现二者都能够提高机械性能,但是含量过高的石墨烯会削弱复合材料的性能;同时骨细胞的培养实验表明碳纳米管能够有效地增加细胞的生长,而石墨烯却没有表现出促进细胞生长的性能。
isdif culttodisperseCNTsinceramicshomogeneously.[12]solutionfor18h,washedwithdistilledwateruntilthepHGNshavingoneormoregraphenelayersarealternative llersvaluereached7[29].GO akes(Grafguard220–50N)fromforreinforcingnanocomposites.TheYoung’smodulusofGrafTechInternational(Ohio,USA)weresubjectedtoagrapheneisestimatedaround0.5–1.0TPa.[13]GNsoffersimplethermal-shockat7008Cfor10s,andthendispersedindistinctadvantagesoverCNTssuchaslowmaterialcostanddistilledwaterundersonicationfor12htoobtainablackGNeaseoffabrication.Naturallyabundantgraphitewithasolution.
layeredstructurecanbetransformedtographiteoxide(GO)uponoxidationinstrongacids.GOhasemergedasanNanocompositePreparation
attractiveprecursorforlarge-scalesynthesisofgraphene-MWNT/HAandGN/HAnanocompositescontaining0.5,basedmaterials.[14]HeatingGOinafurnacegenerally1,1.5,and2wt%nano llerswereprepared.Acid-oxidizedproducesexpandedgraphitethatcanbefurtherexfoliatedMWNTsofagivenloadinglevelandnHAwereindepen-intothinGNsundersonication.[15]GNsarethenincorporateddentlydispersedintowaterundersonication.ThenMWNTintopolymerstoproducenanocompositeswithhighmechan-dispersionwasdropwiseaddedintotheHAsolutionundericalstrengthandgoodelectricalconductivity.[16–19]Littleissonication.Similarly,blackGNdispersionwasdropwiseknownontheeffectofGNadditionsonthestructureandaddedintotheHAsolutionundersonication.MixedMWNT/mechanicalpropertiesofceramics.
HAandGN/HAsolutionswerefurthersonicatedfor2h,Fromtheliterature,graphenepaperspromoteadhesion ltered,anddriedinanoven(508C)for24h.Themixedandproliferationofosteoblasts.[20]Thegraphene/chitosancompositemixturesweresinteredusingasparkplasmananocompositesalsoexhibitgoodcellbiocompatibility.[21]sinteringsystem(SyntexmodelSPS-825)viaaninitialheatingSimilarly,CNTsalsoexhibitexcellentbiocompatibilityandofthechamberto9008Catarateof1008CminÀ1for2min,andpromoteosteoblastadhesion.[22–24]However,metalcatalystthenincreasedto10008Cfor1minunderapressureofparticlesentrappedinsideCNTsmayaffectbiologicalcell40MPa.Finally,thespecimenswerecooledtoroomresponses.[25]Thepuri cationprocessforremovingmetaltemperatureintheSPSchamber.SinteredproductsofcatalystsinCNTsisquitetime-consuming.Inthisregard,high20mmdiameterand5mmthicknesswerecutintosectionspurityGNscanre ectgenuineresponsesofbiologicalcells.withtheirsurfacesalignedparalleltothepressuredirection.ThosestudiesdescribedabovearemainlyconcernedwiththecellresponsesofCNTsandGNs.Therefore,properunder-MaterialsCharacterization
standingofthestructuralbehaviorandbiocompatibilityofThemorphologyofGNswasexaminedina eld-emissionnHAcompositescontaininglowloadinglevelsofCNTsandscanningelectronmicroscope(SEM)(JeolJSM6335).TheGNsisnecessaryfortheirfutureapplicationsinorthopedics.structureofsinteredHA,MWNT/HA,andGN/HAnano-ThedevelopmentofnovelGN/HAandCNT/HAnanocom-compositesweredeterminedwithanautomaticX-raypositesrequirestheuseofsparkplasmasintering(SPS)fordiffractometer(Siemens)equippedwithNi- lteredCuKaretaining negrainsizes.SPSisaneffectivetechniqueforradiation.ThemorphologyofsinteredMWNT/HAandGN/sinteringnanoceramicsatlowertemperaturesforshortHAnanocompositeswasobservedinaSEM.
periodsoftime.[26–29]Inapreviousstudy,wereportedtheThree-pointbendingspecimenswithadimensionofformationofpreferentiallyorientedHAgrainsinmultiwalled1Â2Â15mm3wereloadedinanInstrontester(model1CNT(MWNT)/HAcompositesduetotheSPSprocessing.[30]196)underacrossheadspeedof0.02mmminÀ1.ThreeThepresentstudyreportsthefabrication,propertycharacter-specimensofeachcompositionweretested.
ization,bioactivityandbiocompatibilityofGN/HAcompo-sitesdesignedforload-bearingimplantapplications.TotheCellMorphology
bestofourknowledge,thereisnopublishedworkreportingMouseosteoblast(MC3T3-E1)cellswereusedforcultiva-theeffectofGNadditionsonthestructure,mechanicaltiononsinteredHA,MWNT/HA2/98,andGN/HA2/98behavior,andbiocompatibilityofSPS-preparedHAcompo-specimens.Thespecimenswithadimensionof0.5Â2Âsites.Themechanicalandbiocompatibilitycharacteristicsof4.5mmwerecutfromsintereddiscs.ThecellswereculturedtheMWNT/HAcompositesfabricatedbySPSarealsoonthesespecimens(n¼3)atadensityof1Â104cellscmÀ2,inaddressedanddiscussed.highDulbecco’sModi edEagleMedium(DMEM,ThermoScienti c)supplementedwith10%v/vfetalbovineserumExperimental
(FBS),antibiotics(100UmLÀ1ofpenicillinand100mgmLÀ1ofstreptomycin).Priortocultivation,thespecimenswereMaterials
sterilizedwith70%ethanolaqueoussolutionandphospha-SyntheticHAnanorodswithanaspectratioof%3werete-bufferedsaline(PBS)solution.The96-wellcellcultureplatepurchasedfromNanjingEmperorNanoMaterialsCo.wasincubatedat378Cinahumidi edatmosphereof5%(Nanjing,China).Multiwalledcarbonnanotubes(MWNTs)CO2/95%air.Afterseedingfor1and3d,thespecimenswerewereobtainedfromNanostructured&AmorphousMaterialsremovedfromthewell,rinsedinPBS,treatedwith10%Inc.(Texas,USA).TodisperseMWNTsuniformlyintheHAformaldehydesolutionto xtheattachedcells.Finally,theymatrix,thetubeswere rstimmersedin60%HNO3boiling
weredehydratedinaseriesofsolutionswithincreasing

ADVANCEDENGINEERINGMATERIALS2011,13,No.4ß2011WILEY-VCHVerlagGmbH&Co.KGaA,Weinheimdoc.guandang.net
337
COMMUNICATION
646 Chemistry Letters Vol.32, No.7 (2003) Fabrication of Hydroxyapatite Sintered Bodies with c Axis Orientation Kazushi Ohta,? Masanori Kikuchi, and ...
00 Electrodeposition of composite hydroxyapatite–...Owing to the inferior mechanical properties of HA...cients of the sintered coating and the substrate...
Hydroxyapatite Spark plasma sintering Mechanical ... carbon materials (such as glassy, graphite, ?...Recently, high density HA and CNTs composite was...