TribologyInternational56(2012)58–65
ContentslistsavailableatSciVerseScienceDirect
TribologyInternational
journalhomepage:doc.guandang.net
TribologicalbehaviorsofSiC/h-BNcompositecoatingatelevatedtemperatures
ChenZishan,LiHejunn,FuQiangang,QiangXinfa
StateKeyLaboratoryofSolidi cationProcessing,Carbon/CarbonCompositesResearchCenter,NorthwesternPolytechnicalUniversity,Xi’an710072,China
articleinfo
Articlehistory:
Received23April2012Receivedinrevisedform21June2012
Accepted27June2012
Availableonline6July2012Keywords:SlidingCoatingWear
Hightemperature
abstract
Inthispaper,thetribologicalbehaviorsofSiC/hexagonalboronnitride(SiC/h-BN)compositecoatingpreparedbypackcementationoncarbon/carbon(C/C)compositeswereinvestigated,comparingwiththoseofSiCcoating.Thewornsurfacesandweardebrisofthesecoatingswereanalyzedbymeansofscanningelectronmicroscopy(SEM)andenergydispersivespectroscopy(EDS).Theresultsshowthattheh-BNadditioncanstabilizethefrictioncoef cientofSiCcoatingatroomtemperature.At6001Cthetribologicalbehaviorsofbothcoatingsshowedsimilarfeaturewithhighfrictioncoef cientandnegligiblewearrate.At8001CtheSiCcoatingunderwentseverewear,whiletheSiC/h-BNcompositecoatingexhibitedselflubricityandpossessedlowerfrictioncoef cientandsmallerwearratethanSiCcoating.
&2012ElsevierLtd.Allrightsreserved.
1.Introduction
Carbon/carbon(C/C)compositesexhibitexcellenthigh-tem-peraturemechanicalproperties,lowdensity,andgoodprocessa-bility,whichareconsideredasthemostpromisingcandidatematerialsforthethermalstructurecomponentsinaerospaceandastronauticsapplications[1,2].However,underextremecondi-tions(e.g.hightemperature,vacuum,etc.)whereliquidlubricantsareeitherundesirableorineffectual,frictionusuallyresultsinseriousdamagetotheworkingsurfaces[3–5].SiCcoatingcanprotecttheC/Ccompositesagainstwearandoxidationeffectivelyinextremeconditionsduetoitshighthermalconductivity,excellentcorrosionresistance,goodtribologicalperformanceandgoodchemicalcompatibilitywithcarbonsubstrate[6–10].Nevertheless,thefrictioncoef cientvaluesofSiCmaterialsagainstseveralopposingsurfacesarestillquithighintheunlubricatedconditions[11,12].
ToimprovethetribologicalpropertiesofSiCmaterials,theeffectsofseveralmaterialmodi cationshavebeeninvestigated.Forinstance,ithasbeenreportedthatceramicmaterialswerecoatedwithatribologicalmaterial,suchasdiamond-likecarbon,toimprovethetribologicalproperties[11–13].Anotherwaytoenhancethelubricityofceramicmaterialsisachievedbyincor-poratingsoftparticles,suchasAg,molybdenumdisul de(MoS2)andhexagonalboronnitride(h-BN)[14–17].h-BNisawell-knowninsitulubricatingmaterial,whichhasakindoflamellar
crystallinestructurethatissimilartothoseofgraphiteandMoS2.Moreover,h-BNisoneoffewviablesolidlubricantsthatworkwellattemperaturesupwardsof6001C.Ithasbeenusedasaneffectivesolidlubricantforhightemperatureapplications[18].Carrapichanoetal.[17]reportedthat,atroomtemperature,siliconnitridematerialscanpro tfromtheadditionofh-BNtoimprovetheirtribologicalpropertiesonlyiflowvolumeamounts(10%)wereincorporated.Recently,theresearch[19]revealedthattheadditionofgraphitewithlowcontentofh-BNcanstabilizetribologicalpropertiesofCu-basedpowdermetallurgyfrictioncompositesatroomtemperature.Althoughh-BNexhibitsoutstandinglubricityathightemperature,littleliteraturehasreportedregardingthetribologicalpropertiesofSiCmaterialsaddingwithh-BNathightemperature.
ThepresentworkisaimedatpreparingSiC/h-BNcoatingonC/CcompositesandinvestigatingthetribologicalbehaviorsofthecompositecoatingagainstSiCballfromroomtemperatureto8001C.Theeffectofh-BNonthetribologicalcharacteristicsofcompositecoatingwasanalyzedanddiscussed.2.Experimental
Thespecimens(Ø36mmÂ8mm)usedassubstrateswerecutfrombulktwodimensionalC/Ccompositeswithadensityof1.75g/cm3,andhand-abradedusing400,800and1500gritSiCabrasivepapersinturns,thencleanedbyultrasonicwithethanolanddriedat1001Cfor2h.
SiC/h-BNcompositecoatingwaspreparedbypackcementa-tion,andforcomparison,theSiCcoatingwithouth-BNwasalso
n
Correspondingauthor.Tel.:þ862988495004;fax:þ862988492642.E-mailaddress:lihejun@nwpu.edu.cn(L.Hejun).
0301-679X/$-seefrontmatter&2012ElsevierLtd.Allrightsreserved.doc.guandang.net
Tribological properties of nickel-graphite composite against different counterfaces at elevated 隐藏>> 维普资讯 http://www.cqvip.com Trnatoso ascin fNonerusMeasfr...
of tribological behaviour of TiN, TiCN and CrN at elevated temperatures ˇ ...8. The influence of temperature on coating wear rate, ceramic ball. ...
Tribological behaviors of spot-textured TiN coatings on M2 high-speed steel under boundary lubri_专业资料。维普资讯 http://www.cqvip.com JunlfUiri SineadTc...
tribological properties of Al2O3-polyimide ...made by compression molding at elevated temperature...behaviors of micrometer copper particle- and ...
Influence of heat treatment on tribological behaviors of novel wrought aluminum...can be obtained by adjusting the ageing temperature.When aged at 450隐藏>>...
Mechanical and tribological properties of AlTiN-AlCrBN...At elevated temperatures (500, 700 °C), the ...As temperature is increased to 500 °C, the ...
ZrO2 (YPSZ) coating at elevated temperatures [22...The ZFM10 composite slides against SiC ceramic ...Tribological properties of high temperature self-...
a type of ultra-high-temperature ceramics (UHTCs...retention of strength at elevated temperatures, and...composite coating 3.3 Tribological Properties of ...
reducing gas at elevated temperature and pressure....And the composite powders have a composition of ...coating shows better tribological performance than ...
Elevated temperature fretting fatigue of Ti-17 with surface treatments(2009) ...2.4 Tribological behaviors of SiC/h-BN composite coating at elevated ...