C.Zishanetal./TribologyInternational56(2012)58–6565
Table2
EDSanalysisfordifferentlayersinFig.6c.Region
Silicon(at.%)Carbon(at.%)Oxygen(at.%)A(Inner-layer)41.3729.3629.27B(Inter-layer)36.7613.4549.79C(Outer-layer)
28.43
–
71.57
iseasiertodeformandslip,whichisbene cialtothereductionoffrictioncoef cient.Moreover,twokindsofdebriswereobservedonthewornsurface.Oneissmallrod-shapeddebris(Fig.8e),anotheristhin akes(Fig.8d).Thethin akesdebrisshouldbepeelingfromthecoatingandcounterpart,whichreattachedtothewornsurfaceandformoxide lm.Yettherod-shapeddebrisformedbyrollingoftheoxide lm[25].
Theaboveobservationandanalysiscombiningwiththefric-tioncoef cientcurvecanhelpustogainabetterunderstandingofthefrictionprocess.Atthebeginningofthetest,thehighfrictioncoef cientwascloselyrelatedtodeformationandfrac-tureofasperitiesonthecontactsurfaces.Simultaneously,lotsofdebrisformedandmoredebrisaccumulatedontheweartrackofthecoating.Theh-BNindebrisworkedassolidlubricant,resultinginthedeclineofthefrictioncoef cient.Moreover,thevery nedebrisreattachedtoformoxide lmonthesurfaceowingtothehighambienttemperature(8001C)andtheinduc-tiveeffectoffriction.The lmwhichdecreasedthecontactforceduetoeffectivelyinhibitingfractureandpulloutofSiCgrains,actedasalubricantanddrovetheweartoasteadystate,thereby,causeddrasticdecreaseofthefrictioncoef cient.Asthetestproceeded,moderateliquidB2O3generatedbytheoxidationofh-BNwasgoodforthedensityandintegrityoftheoxide lm[24].Justafterreachingsteadystate,aneffectivelubricating lmhadformedbetweenthecontactsurfaces.
Itcanbefoundthath-BNplayedanimportantroleintheimprovementoftribologicalperformanceofSiCcoatingat8001C.Firstly,thecharacteristicofh-BNthatistheeasycleavageofbasalplanescanaffordalubricouseffectbeforetheformationofoxide lm.Secondly,accordingtoRefs.[24,26],atribo- lmcontainingB2O3canformonthewornsurfaceowingtotheoxidationofh-BNduringweartest.The lmnotonlyprotectsthetribo-couples,butalsolubricatesthewearsurfaces.Thecrosssectionmorphologyofoxide lmisshowninFig.9.Thedenseoxide lmisabout10mminthickness,whichcoversthecoating,andeffectivelyprotectsthecoatingfromthefurtheroxidation.4.Conclusions
SiCcoatingandSiC/h-BNcompositecoatingwerepreparedbypackcementationonC/Ccomposites.ThetribologicalbehaviorsofSiC/h-BNcompositecoatingatelevatedtemperaturewereinvestigated.Themajorresultsaresummarizedasfollows:(1)Thefrictioncoef cientandwearrateofSiC/h-BNcomposite
coatingareequivalentwiththoseofSiCcoatingatroomtemperature.Theh-BNadditioncanstabilizethefrictioncoef cient.Themainwearmechanismismicro-cutremovingandplasticdeforming.
(2)Asthetemperatureroseto6001C,thewearmechanismof
bothcoatingschangedintosevereadhesionwear,resultinginquitehighfrictioncoef cientandstrongdamagetothecounterparts.
(3)At8001C,oxidationanddelaminationarethemainfactorsfor
theSiCcoatingfailure.However,theSiC/h-BNcompositecoatingexhibitsselflubricity.
(4)Theh-BNisbene cialtotheformationofadensetribo- lm
withlamellarstructure.Thetribo- lmcannotonlydecreasethefrictioncoef cientandwearrate,butalsoprotectthecoatingfromthefurtheroxidation.Acknowledgments
ThisworkhasbeensupportedbytheNationalNaturalScienceFoundationofChinaunderGrantnos.51072166and50832004,theProgramforNewCenturyExcellentTalentsinUniversity,theResearchFundofStateKeyLaboratoryofSolidi cationProcessing(NWPU),China(Grantno.25-TZ-2009).References
[1]WestwoodAVK,RandB,LuS.Oxidationresistantcarbonmaterialsderived
fromboronatedcarbon–siliconalloys.Carbon2004;42:3071–80.
[2]CaioCAA,FlorianM,GracaMLA,BressianiJC.KineticstudybyTGAofthe
effectofoxidationinhibitorsforcarbon–carboncomposite.MaterialsScienceandEngineeringA2003;358:298–303.
[3]GuoC,ZhouJS,ZhaoJR.MicrostructureandtribologicalpropertiesofTiCu2Al
intermetalliccompoundcoating.AppliedSurfaceScience2011;257:5885–92.[4]ChildsTHC,MimarogluA.Slidingfrictionandwearupto6001Cofhighspeed
steelsandsiliconnitridesforgasturbinebearings.Wear1993;162–164:890–6.[5]RenSF,MengJH,LuJJ.TribologicalbehaviorofTi3SiC2slidingagainstNi-basedalloysatelevatedtemperatures.TribologyLetters2008;3:129–37.[6]FuQG,LiHJ,ShiXH,LiKZ,SunGD.Siliconcarbidecoatingtoprotectcarbon/
carboncompositesagainstoxidation.ScriptaMaterialia2005;52:923–7.
[7]LiuCD,ChengLF,LuanXL,MeiH.High-temperaturefatiguebehaviorofSiC-coatedcarbon/carboncompositesinoxidizingatmosphere.JournaloftheEuropeanCeramicSociety2009;29:481–7.
[8]ChuYH,FuQG,LiHJ,LiKZ,ZouX,GuCG.In uenceofSiCnanowiresonthe
propertiesofSiCcoatingforC/Ccompositesbetweenroomtemperatureand15001C.CorrosionScience2011;53:3048–52.
[9]RaniDA,YoshizawaY,HyugaH,HiraoK,YamauchiY.Tribologicalbehaviorof
ceramicmaterials(Si3N4,SiCandAl2O3)inaqueousmedium.JournaloftheEuropeanCeramicSociety2004;24:3279–84.
[10]HsuSM,ShenM.Wearpredictionofceramics.Wear2004;256:867–78.
[11]ChoiHJ,BaeHT,LeeJK,NaBC,McNallanMJ,LimDS.Slidingwearofsilicon
carbidemodi edbyetchingwithchlorineatvarioustemperatures.Wear2009;266:214–9.
[12]WangYX,WangLP,XueQJ.Improvingthetribologicalperformancesof
graphite-likecarbon lmonSi3N4andSiCbyusingSiinterlays.AppliedSurfaceScience2011;257:10246–53.
[13]FuRKY,MeiYF,FuMY.Thermalstabilityofmetal-dopeddiamond-like
carbonfabricatedbydualplasmadeposition.DiamondandRelatedMaterials2005;14:1489–93.
[14]TyagiR,XiongDS,LiJL.High-temperaturefrictionandwearofAg/h-BNcontaining
Ni-basedcompositesagainststeel.TribologyLetters2010;40:181–6.
[15]LeonOA,StaiaMH,HintermannHE.WearmechanismofNi-P-BN(h)composite
autocatalyticcoatings.SurfaceandCoatingsTechnology2005;200:1825–9.
[16]XuGZ,ZhouZR,LiuJJ,MaXH.Aninvestigationoffrettingbehaviorofion-platedTiN,magnetron-sputteredMoS2andtheircompositecoatings.Wear1999;225–229:46–52.
[17]CarrapichanoJM,GomesJR,SilvaRF.TribologicalbehaviourofSi3N4-BN
ceramicmaterialsfordryslidingapplications.Wear2002;253:1070–6.
[18]KimuraY,WakabayashiT.Boronnitrideasalubricantadditive.Wear
1999;232:199–206.
[19]ChenBM,BiQL,YangJ,XiaYQ,HaoJC.Tribologicalpropertiesofsolid
lubricants(graphite,hBN)forCubasedP/Mfrictioncomposites.TribologyInternational2008;41:1145–52.
[20]LiWL,TaoNR,HanZ,LuK.Comparisonsofdryslidingtribologicalbehaviors
betweencoarse-grainedandnanocrystallinecopper.Wear2012;274–275:306–12.
[21]ShafferPT.Solubilityofboroninalphasiliconcarbide.MaterialsResearch
Bulletin1970;5:519–21.
[22]CarrereP,LamonJ.CreepbehaviourofaSiC/Si-B-Ccompositewithaself-healingmultilayeredmatrix.JournaloftheEuropeanCeramicSociety2003;23:1105–14.
[23]YiGW,YanFY.Effecthexagonalboronnitrideandcalcinedpetroleumcoke
onfrictionandwearbehaviorofphenolicresin-basedfrictioncomposites.MaterialsScienceandEngineeringA2006;425:330–8.
[24]ErdemirA,BindalC,ZuikerC,SavrunE.Tribologyofnaturallyoccurringboricacid
lmsonboroncarbide.SurfaceandCoatingsTechnology1996;86–87:507–10.[25]MurthyVSR,KobayashiH,TsurekawaS,TamariN.In uenceofhumidityand
dopingelementsonthefrictionandwearofSiCinunlubricatedsliding.TribologyInternational2004;37:353–64.
[26]ChenW,GaoYM,ChenC,XingJD.TribologicalcharacteristicsofSi3N4-hBN
ceramicmaterialsslidingagainststainlesssteelwithoutlubrication.Wear2010;269:241–8.
Tribological properties of nickel-graphite composite against different counterfaces at elevated 隐藏>> 维普资讯 http://www.cqvip.com Trnatoso ascin fNonerusMeasfr...
of tribological behaviour of TiN, TiCN and CrN at elevated temperatures ˇ ...8. The influence of temperature on coating wear rate, ceramic ball. ...
Tribological behaviors of spot-textured TiN coatings on M2 high-speed steel under boundary lubri_专业资料。维普资讯 http://www.cqvip.com JunlfUiri SineadTc...
tribological properties of Al2O3-polyimide ...made by compression molding at elevated temperature...behaviors of micrometer copper particle- and ...
Influence of heat treatment on tribological behaviors of novel wrought aluminum...can be obtained by adjusting the ageing temperature.When aged at 450隐藏>>...
Mechanical and tribological properties of AlTiN-AlCrBN...At elevated temperatures (500, 700 °C), the ...As temperature is increased to 500 °C, the ...
ZrO2 (YPSZ) coating at elevated temperatures [22...The ZFM10 composite slides against SiC ceramic ...Tribological properties of high temperature self-...
a type of ultra-high-temperature ceramics (UHTCs...retention of strength at elevated temperatures, and...composite coating 3.3 Tribological Properties of ...
reducing gas at elevated temperature and pressure....And the composite powders have a composition of ...coating shows better tribological performance than ...
Elevated temperature fretting fatigue of Ti-17 with surface treatments(2009) ...2.4 Tribological behaviors of SiC/h-BN composite coating at elevated ...