C.Xuetal./SolidStateSciences41(2015)52e5553
obtainedinourprocessarecolorlessandtransparent.Particularly,thisprocesscanshapetheproductsaswhiskersinregularcrystalmorphologies,withadiameterofabout10mmandalengthof1mm.
2.Experimentalprocedure2.1.Samplepreparations
CommercialavailableZrO2powderwithpurityof99.9%andgrainsizeof2e4mmwasusedasthestartingmaterial.Inourexperiment,we rstpre-compressedtherawmaterialintoZrO2cylinderswith3.5mmindiameterand1.5mminheight,andtreatedattemperatureof1200 Catnormalpressurefor2h.Thenweputthesampleintothehighpressurecell,andconductedthehighpressuresynthesisprocess.2.2.Highpressureexperiments
Highpressuresynthesisexperimentswerecarriedoutbyusingatwo-stagemultianvilapparatusbasedontheDS6Â8MNcubicpressdevelopedatSichuanUniversity[16].Theanvilsoftungstencarbidecubeswithtruncationedgelengthof8mmwereusedtogeneratepressure,andtheoctahedralsemi-sinteredmagnesia(MgO)with14mmintheedgelengthservedasthepressureme-dium.ThesampleassemblywasdesignedasshowninFig.1.AroundtheTantalumfoilheater,ZrO2tubeswereappliedasthethermalinsulator,andthecenteroftheassemblywas ledwithhexagonalBoronNitride.BetweenthehexagonalBoronNitridecylinderandtheZrO2thermalinsulatorplug,thepretreatedZrO2samplesweresandwiched.Inourexperiments,pressureswereestimatedbasedonthephasetransitionspointsofreferencema-terialsatroomtemperature,andthetemperaturesinthesamplecellweremeasuredusingaB-typethermocouple[17,18].Inatypicalsynthesisprocedure,we rstincreasedthepressureto15GPawithin8h,andthenheatedthesampletoadesiredtem-perature(1800 C)withtheincreasingrateof100 C/min.AfterholdingthesampleunderthepeakP-Tconditionsfor10min,wecooleditdowntoroomtemperaturebyswitchingoffthepowersupply,andthenreleasedthepressureinabout15h.Whenitwasreleasedtoroompressure,wecouldobtaintheneedle-likecrys-tallineproductsbyopeningthesampleassembly.2.3.Samplecharacterizations
Thephasesofthestartingmaterialsandtheproductswere
Fig.1.Sampleassemblyofhighpressureandhightemperaturesynthesis

experiment.
identi edbybothpowderX-raydiffraction(XRD)intheDX-2500X-raydiffractometer,withtheCuKaradiation(l¼0.15406nm),andRaman-scatteringexperiments.Ramanscatteringspectroscopywasobtainedatroomtemperaturebyusingamicro-Ramanspec-trometerinabackscatteringconfiguration.Asolid-statelaser(l¼532nm)wasusedastheexcitationsource.Thelaserbeamwasfocusedontothesample,andthesizeofthelaserspotatthesamplesurfacewasapproximately5mm.Thescatteredsignalwasdispersedwithaspectrometer,anddetectedwithacharge-coupled-devicedetector.Thespatialresolutionwaslessthan1mm,andthespectralresolutionwasabout1cmÀ1.ThemorphologyoftherecoveredsamplestreatedunderHPHTwereobservedusingopticalmicroscope,andfurtherstudiedbyfieldemissionscanningelectronmicroscope.3.Resultsanddiscussion
Afteratypicalsynthesisprocedure,theproductsweretakenoutfromthehighpressureassembly,andtheneedleshapedcrystalscouldbeclearlyidenti ed.AsshowninFig.2(a),abunchoflongandidiomorphicneedle-shapedZrO2whiskerswithsizesupto1mminlengthandas neas10mmindiameterweregrownontheBoronNitridesubstrate.Theboronnitridesubstratesurface

was
Fig.2.OpticalimagesofthepreparedZrO2whiskers:(a)Abunchoflongandidio-morphicneedle-shapedZrO2whiskersgrownontheBoronNitridesubstrate;(b)theneedle-shaped,colorlessandtransparentZrO2whiskers.